Multi-element nano-alloy back light target material, preparation method and application thereof

By loading multi-element nano-alloy particles onto a carbon paper substrate and adjusting the X-ray energy range, the problem of unadjustable energy in existing technologies was solved, enabling efficient broadband X-ray generation and Laue diffraction applications.

CN117647549BActive Publication Date: 2026-11-24UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311663512.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2026-11-24
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

In existing technologies, dynamic Laue diffraction studies based on implosion targets require high backlight laser energy and have an unadjustable X-ray energy range, resulting in the absence of low-energy X-ray spectra and reducing the acquisition efficiency and spatial resolution of Laue diffraction.

Method used

By using a multi-element nano-alloy backlight target material, quasi-continuous broadband X-rays are generated by uniformly loading spherical alloy nanoparticles onto the surface of a carbon paper substrate and utilizing the characteristic X-ray spectrum of high atomic number elements and the confinement effect of nanoparticles to adjust the X-ray energy range.

Benefits of technology

It enables the generation of broadband X-rays with adjustable energy range under lower device requirements, which can be used as a Laue diffraction source to improve the acquisition efficiency and spatial resolution of dynamic Laue diffraction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117647549B_ABST
    Figure CN117647549B_ABST
Patent Text Reader

Abstract

This invention discloses a multi-element nano-alloy backlight target material, its preparation method, and its application, belonging to the field of dynamic broadband X-ray diffraction technology. Specifically, the material consists of quasi-spherical alloy nanoparticles uniformly loaded onto the surface of a carbon paper substrate. These quasi-spherical alloy nanoparticles include at least three high atomic number elements, with each high atomic number element accounting for no less than 5% of the total atomic number. This invention utilizes the rich characteristic X-ray spectrum of high atomic number elements and the confinement effect of nanoparticles to generate broadband quasi-continuous X-rays under pulsed laser driving, which can be used as a Laue diffraction source. Furthermore, the X-ray energy range can be freely adjusted by controlling the composition of the high atomic number elements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of dynamic broadband X-ray diffraction technology, specifically relating to a multi-element nano-alloy backlight target material, its preparation method, and its application. Background Technology

[0002] X-ray diffraction analysis is based on the diffraction effect of X-rays in crystalline materials to analyze the material structure. Since X-ray diffraction follows Bragg's law, inverting the lattice type and cell parameters of a crystalline material from the X-ray diffraction pattern is currently the most direct and reliable technique. Dynamic X-ray diffraction involves inserting an X-ray pulse at a specific moment during high-pressure loading and obtaining information about the lattice evolution of the material at that moment through the inversion and analysis of the instantaneous diffraction pattern. As early as 1969, Johnson et al. began to attempt to use short-pulse X-ray diffraction to measure the mechanical behavior of single crystals under impact loading, and in 1970 successfully obtained the dynamic diffraction signal of the (002) crystal plane, opening a completely new path for the real-time characterization of the microstructure evolution of materials under extreme deformation conditions.

[0003] Depending on the X-ray energy range, dynamic X-ray diffraction analysis techniques can be further divided into Bragg diffraction based on monochromatic X-rays and Laue diffraction based on broadband X-rays. Compared with monochromatic diffraction imaging techniques, Laue diffraction can not only acquire richer diffraction spot signals within the same exposure time, thus improving the acquisition efficiency of diffraction signals, but it is also more sensitive to changes in the internal defect structure of crystals at the microscale. The resulting diffraction spot stars and satellite spots can more clearly indicate the occurrence of plastic deformation caused by slip, thereby providing key information such as defect type, density, and spatial distribution.

[0004] In recent years, researchers have utilized the principle of generating pulsed X-rays through the interaction of high-energy lasers with metal targets, using large-scale laser devices as integrated experimental platforms combining loading and diagnostic capabilities. Through rational target device design and selection of backlight target materials, in-situ X-ray measurements of the dynamic loading process have been achieved.

[0005] High-power laser pulses focused on a target surface can generate high-temperature, dense plasma X-ray sources. Utilizing the bremsstrahlung process of high-temperature, high-density plasma in an implosion target compressed to its focal phase, broadband, smooth, continuous-spectrum X-rays in the 10–25 keV energy range can be produced. The inherent characteristics of the implosion process determine that the generated X-ray source has short pulses (<200 ps), small size (<100 μm), and high brightness, making it suitable for diagnosing dynamic Laue diffraction. However, dynamic Laue diffraction studies based on implosion targets require very high backlight laser energy (>20 kJ), and the X-ray energy range is not adjustable (determined by the implosion physics mechanism, typically 10–25 keV). The absence of low-energy X-ray spectra (<10 keV) can reduce the acquisition efficiency and spatial resolution of Laue diffraction to some extent, leading to the loss of diffraction signals from slip feature planes (usually close-packed crystallographic planes with large interplanar spacing; the appearance of first-order Laue diffraction signals depends on the lower energy limit of the X-rays).

[0006] Nanosecond lasers interacting with solid targets can generate X-rays in the keV energy range, including K-shell X-ray sources for low to medium atomic number (low Z) target materials, L-shell X-ray sources for medium atomic number (medium Z) target materials, and M-shell X-ray sources for high atomic number (high Z) target materials. X-rays generated by this mechanism have a narrow energy distribution and typically exhibit good monochromaticity, making them widely used in dynamic X-ray imaging and diffraction experiments. In 2010, Suggit et al. first constructed a quasi-continuous broadband X-ray source driven by a 250J laser by sequentially depositing Ti, V, Pd, Ag, Sn, CsI, and Sm metals on a 10μm plastic substrate. Utilizing the concept of recombination of characteristic X-ray spectra of multiple solid target elements, they successfully applied this source to the study of impact deformation behavior in single-crystal Cu, observing crystal plane rotation caused by double-slip behavior.

[0007] Compared with the previous two types of techniques, the dynamic broadband X-ray diagnostic method based on multi-metal targets has lower requirements for equipment, and the X-ray energy range can be freely adjusted by controlling the composition of metal elements. Therefore, it can adjust the diffraction wavelength for specific physical problems and has greater room for development and improvement. Summary of the Invention

[0008] To address the problems existing in the prior art, this invention proposes a multi-element nano-alloy backlight target material, its preparation method, and its application, which can be excited to form a more ideal Laue diffraction source.

[0009] The technical solution adopted in this invention is as follows:

[0010] A multi-element nano-alloy backlight target material, specifically, quasi-spherical alloy nanoparticles uniformly loaded on the surface of a carbon paper substrate; the quasi-spherical alloy nanoparticles include at least three high atomic number (high Z) elements, and the atomic percentage of each high atomic number element is not less than 5%.

[0011] Furthermore, the high atomic number element is Se, La, Re, Sm, Dy, Yb or Pt.

[0012] Furthermore, the particle size of the spherical alloy nanoparticles is 50–500 nm.

[0013] Furthermore, by employing different combinations of high atomic number elements, the energy range of the excited quasi-continuous X-rays can be adjusted.

[0014] The preparation method of the multi-element nano-alloy backlight target material includes the following steps:

[0015] Step 1: Determine all high atomic number elements included in the nano-alloy, dissolve the chlorides corresponding to each high atomic number element in anhydrous ethanol, and mix them to obtain a multi-component mixed precursor solution.

[0016] Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride;

[0017] Step 3: Carbothermic shock reaction is carried out on carbon paper substrate loaded with alloy chloride under a protective atmosphere to obtain multi-element nano-alloy backlight target material.

[0018] Furthermore, the concentration of the chlorides corresponding to each high atomic number element in step 1 after dissolving in anhydrous ethanol is 500 mol / L.

[0019] Furthermore, the specific process of the carbothermal shock reaction in step 3 is as follows: an instantaneous voltage of 15-25V is applied to the carbon paper substrate per square centimeter. The current through the carbon paper substrate generates Joule heating, which in turn generates a high-temperature pulse, causing the loaded alloy chloride to decompose at high temperature. Among them, the Cl element is vaporized and volatilized, and the high atomic number elements are mutually dissolved in the reducing environment on the surface of the carbon paper substrate to form alloy nanodroplets. Since the pulse time of the instantaneous voltage is limited to less than 1 second, the molten alloy nanodroplets do not have time to migrate and grow. After the power is turned off, the carbon paper substrate cools rapidly, and spherical alloy nanoparticles are formed on the surface.

[0020] This invention also provides the application of the multi-element nano-alloy backlight target material in a dynamic broadband X-ray source.

[0021] Furthermore, the cut multi-element nano-alloy backlight target material is installed in the optical path of a high-energy pulsed laser platform, and quasi-continuous broadband X-rays are generated under the drive of a pulsed laser of 1.0–3.2 kJ.

[0022] The beneficial effects of this invention are as follows:

[0023] 1. This invention proposes a multi-element nano-alloy backlight target material, specifically a spherical alloy nanoparticle uniformly loaded on the surface of a carbon paper substrate and comprising at least three high atomic number elements. Utilizing the rich characteristic X-ray spectrum of high atomic number elements and the confinement effect of nanoparticles, quasi-continuous X-rays can be generated under the drive of a pulsed laser, which can be used as a Laue diffraction source. Furthermore, the X-ray energy range can be freely adjusted by controlling the composition of high atomic number elements.

[0024] 2. When the multi-element nano-alloy backlight target material obtained in this invention is applied to a dynamic broadband X-ray source, it is driven by a 1.0 to 3.2 kJ pulsed laser in the optical path of a high-energy pulsed laser platform. It does not need to undergo the implosion process of a gas sphere, thus requiring less equipment. Furthermore, the diffraction wavelength range can be adjusted for specific physical problems, showing great application potential. Attached Figure Description

[0025] Figure 1 The image shows the XRD (X-ray diffraction) pattern of the SeDyReLaYb nanoalloy backlight target material prepared in Example 1.

[0026] Figure 2 SEM (scanning electron microscope) image of the SeDyReLaYb nanoalloy backlight target material prepared in Example 1;

[0027] Figure 3 The elemental distribution diagram of the SeDyReLaYb nanoalloy backlight target material prepared in Example 1 is shown below.

[0028] Figure 4 The image shows the XRD pattern of the SeSmDyReLaYbPt nanoalloy backlight target material prepared in Example 2.

[0029] Figure 5 SEM image of the SeSmDyReLaYbP nanoalloy backlight target material prepared in Example 2;

[0030] Figure 6 The elemental distribution diagram of the SeSmDyReLaYbP nanoalloy backlight target material prepared in Example 2 is shown below.

[0031] Figure 7 SEM image of the SmDyLaYb nano-alloy backlight target material prepared in Example 3;

[0032] Figure 8 The elemental distribution diagram of the SmDyLaYb nanoalloy backlight target material prepared in Example 3 is shown below.

[0033] Figure 9 The quasi-continuous X-ray spectrum produced by the SmDyLaYb nanoalloy backlight target material prepared in Example 3;

[0034] Figure 10 SEM image of the DyLaYb nano-alloy backlight target material prepared in Example 4;

[0035] Figure 11 The elemental distribution diagram is shown for the DyLaYb nanoalloy backlight target material prepared in Example 4. Detailed Implementation

[0036] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in conjunction with the following specific embodiments and with reference to the accompanying drawings.

[0037] Example 1

[0038] This embodiment prepares a multi-element nano-alloy backlight target material, specifically a selenium-dysprosium-ruthenium-lanthanum-ytterbium (SeDyReLaYb) nano-alloy backlight target material, including the following steps:

[0039] Step 1: Weigh 220mg SeCl4, 393mg ReCl4, 377mg DyCl4, 372mg LaCl4, and 388mg YbCl4, and dissolve them in 2mL of anhydrous ethanol to obtain anhydrous ethanol solutions of each raw material. Measure anhydrous ethanol solutions of each raw material in equal volume ratio, mix them evenly, and obtain a multi-component mixed precursor solution.

[0040] Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride;

[0041] Step 3: Carbothermic shock reaction is performed on the carbon paper substrate loaded with alloy chloride under an argon atmosphere. A transient voltage of 20V is applied to the carbon paper substrate per square centimeter for a pulse duration of 400ms. After instantaneous heating and rapid cooling, SeDyReLaYb alloy nanoparticles are uniformly loaded on the surface of the carbon paper substrate, thereby obtaining the SeDyReLaYb nano-alloy backlight target material.

[0042] The SeDyReLaYb nanoalloy backlight target material obtained in this embodiment was subjected to XRD, SEM, and TEMEDS (energy-dispersive electron microscopy) tests. Figure 1The XRD pattern shown indicates that the SeDyReLaYb alloy nanoparticles exhibit diffraction peaks in the 35–45° range, primarily indicating a cubic crystal structure. According to... Figure 2 The SEM images show that the obtained SeDyReLaYb alloy nanoparticles are uniformly distributed on the surface of the carbon paper substrate, with a spherical morphology and a particle size of 50–300 nm. Figure 3 The elemental distribution diagram shows that Se, Dy, Re, La and Yb elements are uniformly distributed in the SeDyReLaYb alloy nanoparticles.

[0043] The atomic percentages of Se, Dy, Re, La, and Yb in the SeDyReLaYb alloy nanoparticles obtained in this embodiment are shown in Table 1.

[0044] Table 1

[0045] element Se La Dy Yb Re Total Atomic percentage 17.2 18.3 21.3 26.7 16.5 100

[0046] Example 2

[0047] This embodiment prepares a multi-element nano-alloy backlight target material, specifically a selenium-strontium-dysprosium-ruthenium-lanthanum-ytterbium-platinum (SeSmDyReLaYbPt) nano-alloy backlight target material, including the following steps:

[0048] Step 1: Weigh 220mg SeCl4, 365mg SmCl4, 377mg DyCl4, 393mg ReCl4, 372mg LaCl4, 388mg YbCl4, and 518mg H2PtCl6, and dissolve them in 2mL of anhydrous ethanol to obtain anhydrous ethanol solutions of each raw material. Measure an equal volume ratio of the anhydrous ethanol solutions of each raw material, mix them thoroughly, and obtain a multi-component mixed precursor solution.

[0049] Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride;

[0050] Step 3: Carbothermic shock reaction is performed on the carbon paper substrate loaded with alloy chloride under an argon atmosphere. A transient voltage of 15V is applied to the carbon paper substrate per square centimeter for a pulse duration of 600ms. After instantaneous heating and rapid cooling, SeSmDyReLaYbPt alloy nanoparticles are uniformly loaded on the surface of the carbon paper substrate, thereby obtaining the SeSmDyReLaYbPt nanoalloy backlight target material.

[0051] The SeSmDyReLaYbPt nanoalloy backlight target material obtained in this embodiment was subjected to XRD, SEM, and TEMEDS tests. Figure 4The XRD pattern shown indicates that the SeSmDyReLaYbPt alloy nanoparticles exhibit diffraction peaks in the 35–45° range, primarily indicating a cubic crystal structure. According to... Figure 5 The SEM images show that the obtained SeSmDyReLaYbPt alloy nanoparticles are uniformly distributed on the surface of the carbon paper substrate, with a spherical morphology and a particle size of 50–200 nm. Figure 6 The elemental distribution diagram shows that Se, Sm, Dy, Re, La, Yb and Pt elements are uniformly distributed in the SeSmDyReLaYbPt alloy nanoparticles.

[0052] The atomic percentages of Se, Sm, Dy, Re, La, Yb, and Pt elements in the SeSmDyReLaYbPt alloy nanoparticles obtained in this embodiment are shown in Table 2.

[0053] Table 2

[0054] element Se La Sm Dy Yb Re Pt Total Atomic percentage 9.2 17.7 19.1 14.6 21.2 11.3 6.9 100

[0055] Example 3

[0056] This embodiment prepares a multi-element nano-alloy backlight target material, specifically a strontium-dysprosium-lanthanum-ytterbium (SmDyLaYb) nano-alloy backlight target material, including the following steps:

[0057] Step 1: Weigh 365mg SmCl4, 377mg DyCl4, 372mg LaCl4, and 388mg YbCl4, and dissolve them in 2mL of anhydrous ethanol to obtain anhydrous ethanol solutions of each raw material. Measure anhydrous ethanol solutions of each raw material in equal volume ratios, mix them evenly, and obtain a multi-component mixed precursor solution.

[0058] Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride;

[0059] Step 3: Carbothermic shock reaction is performed on the carbon paper substrate loaded with alloy chloride under an argon atmosphere. A transient voltage of 25V is applied to the carbon paper substrate per square centimeter, and the pulse time is 100ms. After instantaneous heating and rapid cooling, SmDyLaYb alloy nanoparticles are uniformly loaded on the surface of the carbon paper substrate, thereby obtaining the SmDyLaYb nano-alloy backlight target material.

[0060] The SmDyLaYb nano-alloy backlight target material obtained in this embodiment was subjected to SEM and TEMEDS tests. Figure 7 The SEM image shown reveals that the obtained SmDyLaYb alloy nanoparticles are uniformly distributed on the surface of the carbon paper substrate, exhibiting a near-spherical morphology with a particle size ranging from 50 to 250 nm. Figure 8The elemental distribution diagram shows that Sm, Dy, La and Yb elements are uniformly distributed in the SmDyLaYb alloy nanoparticles.

[0061] The atomic percentages of Sm, Dy, La, and Yb elements in the SmDyLaYb alloy nanoparticles obtained in this embodiment are shown in Table 3.

[0062] Table 3

[0063] element Sm La Dy Yb Total Atomic percentage 28.8 20.3 23.2 27.7 100

[0064] The SmDyLaYb nanoalloy backlight target material obtained in this embodiment was applied to a dynamic broadband X-ray source. Specifically, the cut SmDyLaYb nanoalloy backlight target material was installed in the optical path of a high-energy pulsed laser platform. Using a LiF single crystal with a thickness of more than 100 μm as a standard sample, its X-ray spectral characteristics were tested. Under the driving force of a pulsed laser of 1.0–3.2 kJ, a quasi-continuous broadband X-ray with an energy range of 2.97–10.01 keV was generated. Figure 9 As shown, a relatively ideal Laue diffraction source was formed.

[0065] Example 4

[0066] This embodiment prepares a multi-element nano-alloy backlight target material, specifically a dysprosium-lanthanum-ytterbium (DyLaYb) nano-alloy backlight target material, including the following steps:

[0067] Step 1: Weigh 377mg DyCl4, 372mg LaCl4, and 388mg YbCl4, and dissolve them in 2mL of anhydrous ethanol to obtain anhydrous ethanol solutions of each raw material. Measure anhydrous ethanol solutions of each raw material in equal volume ratio, mix them evenly, and obtain a multi-component mixed precursor solution.

[0068] Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride;

[0069] Step 3: Carbothermic shock reaction is performed on the carbon paper substrate loaded with alloy chloride under an argon atmosphere. A transient voltage of 20V is applied to the carbon paper substrate per square centimeter for a pulse duration of 300ms. After instantaneous heating and rapid cooling, DyLaYb alloy nanoparticles are uniformly loaded on the surface of the carbon paper substrate, thereby obtaining DyLaYb nano-alloy backlight target material.

[0070] The DyLaYb nano-alloy backlight target material obtained in this embodiment was subjected to SEM and TEMEDS tests. Figure 10 The SEM image shown reveals that the obtained DyLaYb alloy nanoparticles are uniformly distributed on the surface of the carbon paper substrate, exhibiting a near-spherical morphology with a particle size ranging from 50 to 250 nm. Figure 11 The elemental distribution diagram shows that Dy, La, and Yb elements are uniformly distributed in the DyLaYb alloy nanoparticles.

[0071] The atomic percentages of Dy, La, and Yb elements in the DyLaYb alloy nanoparticles obtained in this embodiment are shown in Table 4.

[0072] Table 4

[0073] element La Dy Yb Total Atomic percentage 25.7 35.7 39.2 100

[0074] The above embodiments are only for illustrating the principles and advantages of the present invention, and are not intended to limit the present invention. They are only for helping to understand the principles of the present invention. The scope of protection of the present invention is not limited to the above configurations and embodiments. Those skilled in the art can make various other specific modifications and combinations based on the disclosed technology without departing from the essence of the present invention, but they are still within the scope of protection of the present invention.

Claims

1. A method for preparing a multi-element nano-alloy backlight target material, characterized in that, Includes the following steps: Step 1: Determine all high atomic number elements included in the nano-alloy, dissolve the chlorides corresponding to each high atomic number element in anhydrous ethanol, and mix them to obtain a multi-component mixed precursor solution. Step 2: Add the multi-component mixed precursor solution dropwise onto the carbon paper substrate and dry it at 50°C to obtain the carbon paper substrate loaded with alloy chloride; Step 3: Carbothermic shock reaction is carried out on carbon paper substrate loaded with alloy chloride under a protective atmosphere to obtain multi-element nano-alloy backlight target material.

2. The preparation method according to claim 1, characterized in that, The specific process of the carbon thermal shock reaction in step 3 is as follows: an instantaneous voltage of 15~25 V is applied to the carbon paper substrate per square centimeter, and the pulse time of the instantaneous voltage is limited to within 1 s. After the power is turned off, the carbon paper substrate cools rapidly, and spherical alloy nanoparticles are formed on the surface.

3. The preparation method according to claim 2, characterized in that, The obtained multi-element nano-alloy backlight target material is specifically a spherical alloy nanoparticle uniformly loaded on the surface of a carbon paper substrate, including at least three high atomic number elements, and the atomic percentage of each high atomic number element is not less than 5%.

4. The preparation method according to claim 3, characterized in that, The high atomic number element is Se, La, Re, Sm, Dy, Yb or Pt.

5. The preparation method according to claim 3, characterized in that, The particle size of the spherical alloy nanoparticles is 50~500 nm.

6. The preparation method according to claim 3, characterized in that, The energy range of excited quasi-continuous X-rays can be adjusted by using different combinations of high atomic number elements.

7. The application of the multi-element nano-alloy backlight target material obtained by the preparation method according to any one of claims 1 to 6 in a dynamic broadband X-ray source.