Ultraviolet light emitting diode epitaxial wafer and preparation method therefor, light emitting diode
By using a β-Ga₂O₃-graphene composite layer and annealing treatment in the epitaxial wafer of an ultraviolet light-emitting diode, the problem of low activation efficiency of P-type dopants was solved, achieving efficient ohmic contact and low operating voltage, thereby improving luminous efficiency and carrier migration capability.
Patent Information
- Application Number
- CN202311509843.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-14
AI Technical Summary
The low activation efficiency of the P-type dopant Mg in existing AlGaN-based ultraviolet LEDs leads to insufficient holes, reduced radiative recombination efficiency, and low internal quantum efficiency, making it difficult to form ohmic contacts with low operating voltage and affecting luminous efficiency.
A β-Ga₂O₃-graphene composite layer was used as an electron blocking layer and a P-type semiconductor layer. An annealing process was used to form a GaSiC composite, which reduced the oxygen vacancy concentration and improved the carrier migration ability. Furthermore, a high hole concentration P-type contact layer was formed by Mg doping to reduce the contact resistance.
It improves the luminous efficiency of ultraviolet light-emitting diodes, reduces the operating voltage, enhances the ohmic contact effect, improves the carrier migration capability, and reduces the contact resistance.
Smart Images

Figure CN117650211B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to an ultraviolet light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology
[0002] Over the past decade, AlGaN materials have garnered significant attention due to their immense potential applications in ultraviolet (UV) optoelectronic devices. UV LEDs possess characteristics such as high photon energy, short wavelength, small size, low power consumption, long lifespan, and environmental friendliness, leading to their wide application in high color rendering index white light illumination, high-density optical data storage, sensors, offset printing, and air purification. However, the development of AlGaN-based UV LEDs faces numerous technical challenges. For instance, the relatively low effective mass of electrons results in high mobility, causing many electrons to easily overflow through quantum wells into the P-type layer. Ideal N-type and P-type materials are prerequisites for the application of various semiconductor materials and the foundation for the optimal performance of various semiconductor devices. While N-type doping technology is relatively mature for AlGaN-based UV LEDs already in commercial production, P-type doping remains a significant obstacle to their further development. Furthermore, p-type doping of high-Al content AlGaN materials is particularly challenging. The low activation efficiency of the dopant Mg leads to insufficient holes, reduced radiative recombination efficiency, low internal quantum efficiency, and decreased luminous efficiency. The Mg doping concentration and hole concentration of p-type AlGaN-based materials are crucial parameters directly affecting the luminous efficiency of the devices. The acceptor (Mg) impurities in p-type AlGaN-based materials are difficult to ionize, resulting in a low hole concentration. Moreover, the high work function of p-type AlGaN makes it difficult to find metal electrodes to form ohmic contacts with it. Obtaining p-type materials with high hole concentration and high hole mobility, achieving low p-type ohmic contacts and high luminous efficiency, has been a key obstacle to the further development of ultraviolet light-emitting diodes. Therefore, it is necessary to conduct in-depth research on how to improve the problems existing in the aforementioned p-type materials. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer of an ultraviolet light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the ultraviolet light-emitting diode and reduce the operating voltage.
[0004] Another technical problem that this invention aims to solve is to provide an ultraviolet light-emitting diode with high luminous efficiency and low operating voltage.
[0005] To address the aforementioned problems, this invention discloses an epitaxial wafer for an ultraviolet light-emitting diode, comprising a substrate and, sequentially disposed on the substrate, a buffer layer, an undoped AlGaN layer, an N-type semiconductor layer, a multiple quantum well layer, an electron blocking layer, a P-type semiconductor layer, and a P-type contact layer; characterized in that the electron blocking layer is a β-Ga2O3-graphene composite layer, the P-type semiconductor layer is a first P-type β-Ga2O3-graphene composite layer, and the P-type contact layer is a second P-type β-Ga2O3-graphene composite layer.
[0006] As an improvement to the above technical solution, the P-type dopant element in the first P-type β-Ga2O3-graphene composite layer is Mg, and the Mg doping concentration is 1×10⁻⁶. 19 cm -3 -1×10 20 cm -3 ;
[0007] The second p-type β-Ga2O3-graphene composite layer has Mg as the p-type dopant, and the Mg doping concentration is 1×10⁻⁶. 20 cm -3 -1×10 21 cm -3 .
[0008] As an improvement to the above technical solution, the thickness of the second P-type β-Ga2O3-graphene composite layer is less than the thickness of the first P-type β-Ga2O3-graphene composite layer.
[0009] As an improvement to the above technical solution, the thickness of the β-Ga2O3-graphene composite layer is 10nm-80nm, the thickness of the first P-type β-Ga2O3-graphene composite layer is 20nm-80nm, and the thickness of the second P-type β-Ga2O3-graphene composite layer is 5nm-40nm.
[0010] As an improvement to the above technical solution, the β-Ga2O3-graphene composite layer is obtained by annealing a β-Ga2O3 layer;
[0011] The first P-type β-Ga2O3-graphene composite layer is obtained by annealing the first P-type β-Ga2O3 layer;
[0012] The second P-type β-Ga2O3-graphene composite layer is obtained by annealing the second P-type β-Ga2O3 layer.
[0013] As an improvement to the above technical solution, after the β-Ga2O3 layer is grown, the temperature is first maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr, and TMGa, SiH4, and C2H4 are continuously introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm, with an introduction time of 1 min-3 min. Then, annealing is carried out in an H2 atmosphere at a temperature of 1500℃-1700℃, an annealing chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min, thus obtaining the β-Ga2O3-graphene composite layer.
[0014] After the first P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm. The introduction time is 1 min-3 min. Annealing is then performed in an H2 atmosphere at a temperature of 1500℃-1700℃, a chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min. This yields the first P-type β-Ga2O3-graphene composite layer.
[0015] After the second P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm. The introduction time is 1 min-3 min. Annealing is then performed in an H2 atmosphere at a temperature of 1500℃-1700℃, a chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min. This yields the second P-type β-Ga2O3-graphene composite layer.
[0016] As an improvement to the above technical solution, the thickness of the β-Ga2O3 layer is 20nm-100nm;
[0017] The thickness of the first P-type β-Ga2O3 layer is 30nm-100nm;
[0018] The thickness of the second P-type β-Ga2O3 layer is 10nm-50nm.
[0019] Accordingly, the present invention also discloses a method for preparing an ultraviolet light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned ultraviolet light-emitting diode epitaxial wafer, comprising:
[0020] A substrate is provided on which a buffer layer, an undoped AlGaN layer, an N-type semiconductor layer, a multiple quantum well layer, an electron blocking layer, a P-type semiconductor layer, and a P-type contact layer are sequentially grown; the electron blocking layer includes a β-Ga2O3-graphene composite layer, the P-type semiconductor layer includes a first P-type β-Ga2O3-graphene composite layer, and the P-type contact layer includes a second P-type β-Ga2O3-graphene composite layer.
[0021] As an improvement to the above technical solution, the β-Ga2O3-graphene composite layer is obtained by annealing the β-Ga2O3 layer. The growth temperature of the β-Ga2O3 layer is 1100℃-1200℃, the growth pressure is 100 torr-200 torr, and during growth, O2 is introduced as the O source and TMGa is introduced as the Ga source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm.
[0022] The first P-type β-Ga2O3-graphene composite layer is obtained by annealing the first P-type β-Ga2O3 layer. The growth temperature of the first P-type β-Ga2O3 layer is 1100℃-1200℃, the growth pressure is 100 torr-200 torr, and during growth, O2 is introduced as the O source, TMGa is introduced as the Ga source, and Cp2Mg is introduced as the Mg source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm.
[0023] The second P-type β-Ga2O3-graphene composite layer is obtained by annealing the second P-type β-Ga2O3 layer. The growth temperature of the second P-type β-Ga2O3 layer is 1100℃-1200℃, and the growth pressure is 100 torr-200 torr. During growth, O2 is introduced as the O source, TMGa is introduced as the Ga source, and Cp2Mg is introduced as the Mg source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm.
[0024] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned ultraviolet light-emitting diode epitaxial wafer.
[0025] Implementing this invention has the following beneficial effects:
[0026] 1. In the epitaxial wafer of the ultraviolet light-emitting diode of the present invention, the electron blocking layer comprises a β-Ga2O3-graphene composite layer, the P-type semiconductor layer comprises a first P-type β-Ga2O3-graphene composite layer, and the P-type contact layer comprises a second P-type β-Ga2O3-graphene composite layer. First, the electron blocking layer, P-type semiconductor layer, and P-type contact layer of the present invention are all made of β-Ga2O3 and graphene composite materials. There is almost no lattice mismatch between Ga2O3 and AlGaN materials, resulting in good crystal quality and improved diode luminous efficiency. Second, Ga2O3 has a work function of 4.0 eV, which allows for good matching with metal electrodes to form ohmic contacts, reducing the operating voltage. Finally, graphene materials provide a two-dimensional C atomic layer structure, improving carrier migration capability, facilitating hole migration to the quantum well, improving luminous efficiency, and also acting as a current spreader, reducing contact resistance.
[0027] In the epitaxial wafer of the ultraviolet light-emitting diode of the present invention, the P-type doping concentration of the second P-type β-Ga2O3-graphene composite layer is less than that of the first P-type β-Ga2O3-graphene composite layer. The higher P-type doping concentration of the first P-type β-Ga2O3-graphene composite layer ensures a higher hole concentration; the slightly lower P-type doping concentration of the second P-type β-Ga2O3-graphene composite layer avoids a decrease in surface flatness and ensures better ohmic contact.
[0028] 2. In the epitaxial wafer of the ultraviolet light-emitting diode of the present invention, the thickness of the second P-type β-Ga2O3-graphene composite layer is less than the thickness of the first P-type β-Ga2O3-graphene composite layer. The thickness of the second P-type β-Ga2O3-graphene composite layer should be as thin as possible to further reduce the contact resistance. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the structure of an epitaxial wafer of an ultraviolet light-emitting diode in one embodiment of the present invention;
[0030] Figure 2 This is a flowchart of a method for preparing an epitaxial wafer of an ultraviolet light-emitting diode in one embodiment of the present invention. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0032] refer to Figure 1 The present invention discloses an epitaxial wafer for an ultraviolet light-emitting diode, comprising a substrate 1 and a buffer layer 2, an undoped AlGaN layer 3, an N-type semiconductor layer 4, a multiple quantum well layer 5, an electron blocking layer 6, a P-type semiconductor layer 7 and a P-type contact layer 8 sequentially disposed on the substrate 1.
[0033] In this invention, the electron blocking layer 6 is a β-Ga₂O₃-graphene composite layer, the P-type semiconductor layer 7 is a first P-type β-Ga₂O₃-graphene composite layer, and the P-type contact layer 8 is a second P-type β-Ga₂O₃-graphene composite layer. First, the electron blocking layer 6, the P-type semiconductor layer 7, and the P-type contact layer 8 are all made of β-Ga₂O₃ and graphene composite materials. There is almost no lattice mismatch between Ga₂O₃ and AlGaN materials, resulting in good crystal quality and improved diode luminous efficiency. Second, Ga₂O₃ has a work function of 4.0 eV, which allows it to form an ohmic contact with the metal electrode, reducing the operating voltage. Finally, graphene provides a two-dimensional C atomic layer structure, improving carrier migration and facilitating hole-to-quantum-well migration, thus increasing luminous efficiency and providing current spreading, thereby reducing contact resistance.
[0034] Specifically, the p-type dopant element in the first p-type β-Ga₂O₃-graphene composite layer is Mg, but it is not limited to this. The Mg doping concentration is 1 × 10⁻⁶. 19 cm -3 -5×10 20 cm -3 This ensures a high hole concentration without causing a decrease in lattice quality. Preferably, the Mg doping concentration is 1×10⁻⁶. 19 cm -3 -1×10 20 cm -3 An example is 2×10 19 cm -3 2×10 19 cm -3 2×10 19 cm -3 Or 2×10 19 cm -3 However, it is not limited to this.
[0035] Specifically, the p-type dopant in the second p-type β-Ga₂O₃-graphene composite layer is Mg, but it is not limited to this. The Mg doping concentration is 1 × 10⁻⁶. 20 cm -3 -5×10 21 cm -3 Within this range, the Mg doping concentration ensures good ohmic contact without causing a decrease in lattice quality. Preferably, the Mg doping concentration is 1 × 10⁻⁶. 20 cm -3 -1×10 21 cm -3 An example is 2×10 20 cm -3 4×10 20 cm -3 6×1020 cm -3 Or 8×10 20 cm -3 However, it is not limited to this.
[0036] The thickness of the second P-type β-Ga₂O₃-graphene composite layer is less than the thickness of the first P-type β-Ga₂O₃-graphene composite layer. This configuration allows for further reduction of contact resistance.
[0037] Specifically, the thickness of the β-Ga2O3-graphene composite layer is 10nm-90nm, and within this range, it can effectively block electrons. Preferably, the thickness is 10nm-80nm, with exemplary thicknesses of 20nm, 30nm, 40nm, 50nm, or 60nm, but not limited to these.
[0038] Specifically, the thickness of the first P-type β-Ga2O3-graphene composite layer is 20nm-90nm, preferably 20nm-80nm, and exemplary is 30nm, 40nm, 50nm or 60nm, but not limited thereto.
[0039] Specifically, the thickness of the second P-type β-Ga2O3-graphene composite layer is 5nm-50nm, preferably 5nm-40nm, and exemplary are 10nm, 20nm, 30nm or 35nm, but not limited thereto.
[0040] The β-Ga2O3-graphene composite layer is prepared by annealing the β-Ga2O3 layer; the first P-type β-Ga2O3-graphene composite layer is prepared by annealing the first P-type β-Ga2O3 layer; and the second P-type β-Ga2O3-graphene composite layer is prepared by annealing the second P-type β-Ga2O3 layer. β-Ga₂O₃ material has a high oxygen vacancy concentration and many defects, exhibiting N-type conductivity, which is not conducive to hole migration into the quantum well. Annealing is performed by introducing a Ga source, SiH₄, and C₂H₄ to form a GaSiC composite. Further annealing in an H₂ atmosphere allows Ga atoms in the GaSiC composite to diffuse and combine with oxygen vacancies in the β-Ga₂O₃ material, reducing the oxygen vacancy concentration and resulting in a stable β-Ga₂O₃ material. Simultaneously, due to the high vapor pressure of Si atoms in the GaSiC composite, Si atoms evaporate faster than other components, leaving C atoms that rearrange to form a two-dimensional graphene layer. This improves carrier migration, facilitating hole migration into the quantum well and also acts as a current spreader, reducing contact resistance.
[0041] Specifically, after the β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm, with an introduction time of 1 min-3 min. Annealing is then carried out in an H2 atmosphere at a temperature of 1500℃-1700℃, an annealing chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min, thus obtaining the β-Ga2O3-graphene composite layer.
[0042] Specifically, after the first P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing, with the flow rate of TMGa at 50 sccm-100 sccm, the flow rate of SiH4 at 10 sccm-50 sccm, and the flow rate of C2H4 at 100 sccm-200 sccm, for a duration of 1 min-3 min. Annealing is then carried out in an H2 atmosphere at a temperature of 1500℃-1700℃, a pressure of 0 torr-5 torr in the annealing chamber, and a annealing time of 10 min-30 min. This yields the first P-type β-Ga2O3-graphene composite layer.
[0043] Specifically, after the second P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing, with the flow rate of TMGa at 50 sccm-100 sccm, the flow rate of SiH4 at 10 sccm-50 sccm, and the flow rate of C2H4 at 100 sccm-200 sccm, for a duration of 1 min-3 min. Annealing is then carried out in an H2 atmosphere at a temperature of 1500℃-1700℃, a pressure of 0 torr-5 torr in the annealing chamber, and a annealing time of 10 min-30 min. This yields the second P-type β-Ga2O3-graphene composite layer.
[0044] Specifically, the thickness of the β-Ga2O3 layer is 20nm-120nm, preferably 20nm-100nm, and exemplary thicknesses are 30nm, 40nm, 50nm, 60nm or 80nm, but not limited thereto.
[0045] Specifically, the thickness of the first P-type β-Ga2O3 layer is 30nm-120nm, preferably 30nm-100nm, and exemplary are 40nm, 50nm, 60nm or 80nm, but not limited thereto.
[0046] Specifically, the thickness of the second P-type β-Ga2O3 layer is 10nm-60nm, preferably 10nm-50nm, and exemplary are 20nm, 30nm, 40nm or 45nm, but not limited thereto.
[0047] The substrate 1 can be a sapphire substrate, a silicon substrate, or a silicon carbide substrate, but is not limited to these. A sapphire substrate is preferred.
[0048] The buffer layer 2 may be an AlN layer and / or an AlGaN layer, but is not limited thereto. The thickness of the buffer layer 2 is 20nm-200nm, with exemplary thicknesses of 40nm, 60nm, 80nm, 100nm, 150nm, or 180nm, but is not limited thereto.
[0049] The thickness of the undoped AlGaN layer 3 is 1 μm-3 μm, exemplarily 1 μm, 1.5 μm, 2 μm or 2.5 μm, but not limited thereto. The proportion of Al component is 0.3-0.8%, exemplarily 0.4, 0.5, 0.6 or 0.7, but not limited thereto.
[0050] Among them, the N-type semiconductor layer 4 can be Si-doped Al a Ga 1-a N layers, but not limited to these. The doping concentration of the N-type semiconductor layer 4 is 1×10⁻⁶. 19 cm -3 -1×10 20 cm -3 The thickness is 1μm-3μm, and the proportion of Al component is 0.2-0.6%.
[0051] Among them, the multi-quantum well layer 5 is an alternating stack of Al x Ga 1-x N quantum well layer and Al y Ga 1-y N-quantum barrier layers, stacked with 5-12 cycles. A single Al x Ga 1-x The thickness of the N quantum well layer is 2nm-4nm, and the thickness of a single Al y Ga 1-y The thickness of the N quantum barrier layer is 8nm-20nm. x is 0.1-0.5, y is 0.2-0.7, and x < y.
[0052] Accordingly, refer to Figure 2The present invention also discloses a method for preparing an ultraviolet light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned ultraviolet light-emitting diode epitaxial wafer, and includes the following steps:
[0053] S100: Provides a substrate;
[0054] The substrate is loaded into MOCVD and annealed at 1000℃-1200℃, 150 torr-500 torr, in a hydrogen atmosphere for 5 min-10 min to remove impurities such as particles and oxides from the substrate surface.
[0055] S200: A buffer layer is grown on the substrate;
[0056] Specifically, an AlGaN layer grown by MOCVD or an AlN layer grown by PVD can be used as a buffer layer, but it is not limited to these. Preferably, the AlN layer is grown by PVD, with the PVD equipment sputtering temperature at 400℃-700℃, power at 3000W-5000W, and pressure at 1 torr-10 torr.
[0057] S300: An undoped AlGaN layer is grown on the buffer layer;
[0058] Specifically, undoped AlGaN layers were grown in MOCVD at a temperature of 1050℃-1200℃ and a pressure of 50 torr-100 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; H2 and N2 were used as carrier gases; TMGa was introduced as the Ga source; and TMAl was introduced as the Al source.
[0059] S400: An N-type semiconductor layer is grown on an undoped AlGaN layer;
[0060] Specifically, an N-type semiconductor layer is grown in MOCVD at a temperature of 1100℃-1200℃ and a pressure of 50 torr-100 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and SiH4 is introduced as the N-type doping source; H2 and N2 are used as carrier gases, TMGa is introduced as the Ga source, and TMAl is introduced as the Al source.
[0061] S500: A multi-quantum-well layer is grown on an N-type semiconductor layer;
[0062] Among them, multiple Al atoms are periodically grown using MOCVD. x Ga 1-x N quantum well layer and Al y Ga 1-y An N-quantum barrier layer is obtained, which is equivalent to a multi-quantum well layer. Al x Ga 1-xThe growth temperature of the N quantum well layer is 900℃-1000℃, and the growth pressure is 50 torr-100 torr. Al y Ga 1-y The growth temperature of the N quantum barrier layer is 1000℃-1100℃, and the growth pressure is 50 torr-100 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga source, and TMAl is introduced as the Al source.
[0063] S600: An electron blocking layer is grown on a multi-quantum-well layer;
[0064] Specifically, in one embodiment of the present invention, S600 includes:
[0065] S610: β-Ga2O3 layer is grown on a multi-quantum-well layer;
[0066] Specifically, β-Ga2O3 layers were grown using MOCVD at a growth temperature of 1100℃-1200℃ and a growth pressure of 100 torr-200 torr. During growth, O2 was introduced as the O source and TMGa was introduced as the Ga source. The flow rate of O2 was 100 sccm-300 sccm and the flow rate of TMGa was 50 sccm-100 sccm.
[0067] S620: Anneal the β-Ga2O3 layer;
[0068] Specifically, the β-Ga2O3 layer is annealed in MOCVD to obtain the β-Ga2O3-graphene composite layer.
[0069] S700: A P-type semiconductor layer is grown on an electron blocking layer;
[0070] Specifically, in one embodiment of the present invention, S700 includes:
[0071] S710: The first p-type β-Ga2O3 layer is grown on the electron blocking layer;
[0072] Specifically, the first p-type β-Ga2O3 layer was grown in MOCVD at a temperature of 1100℃-1200℃ and a pressure of 100 torr-200 torr. During growth, O2 was introduced as the O source, TMGa as the Ga source, and Cp2Mg as the Mg source. The flow rate of O2 was 100 sccm-300 sccm, and the flow rate of TMGa was 50 sccm-100 sccm.
[0073] S720: Anneal the first P-type β-Ga2O3 layer;
[0074] Specifically, the first P-type β-Ga2O3 layer is annealed in MOCVD to obtain the first P-type β-Ga2O3-graphene composite layer.
[0075] S800: A P-type contact layer is grown on a P-type semiconductor layer;
[0076] Specifically, in one embodiment of the present invention, S800 includes:
[0077] S810: A second P-type β-Ga2O3 layer is grown on the P-type semiconductor layer;
[0078] Specifically, a second p-type β-Ga2O3 layer was grown in MOCVD at a temperature of 1100℃-1200℃ and a pressure of 100 torr-200 torr. During growth, O2 was introduced as the O source, TMGa as the Ga source, and Cp2Mg as the Mg source. The flow rate of O2 was 100 sccm-300 sccm, and the flow rate of TMGa was 50 sccm-100 sccm.
[0079] S820: Anneal the second P-type β-Ga2O3 layer;
[0080] Specifically, the second P-type β-Ga2O3 layer is annealed in MOCVD to obtain the second P-type β-Ga2O3-graphene composite layer.
[0081] The present invention will be further described below with reference to specific embodiments:
[0082] Example 1
[0083] This embodiment provides an epitaxial wafer for an ultraviolet light-emitting diode, as shown in the reference. Figure 1 It includes a substrate 1 and a buffer layer 2, an undoped AlGaN layer 3, an N-type semiconductor layer 4, a multiple quantum well layer 5, an electron blocking layer 6, a P-type semiconductor layer 7, and a P-type contact layer 8 sequentially disposed on the substrate 1.
[0084] In this design, substrate 1 is a sapphire substrate; buffer layer 2 is an AlN layer with a thickness of 30 nm; undoped AlGaN layer 3 has a thickness of 3 μm and an Al content of 0.5%; and N-type semiconductor layer 4 is Si-doped Al. a Ga 1-a The N-layer has a Si doping concentration of 5 × 10⁻⁶. 19 cm -3 Its thickness is 3μm, and the proportion of Al component is 0.4%.
[0085] Among them, the multi-quantum well layer 5 is an alternating stack of Al x Ga 1-x N quantum well layer (x = 0.4) and Aly Ga 1-y N (y = 0.6) quantum barrier layers, stacking period number 9, single Al x Ga 1-x The thickness of the N quantum well layer is 3 nm, and a single Al y Ga 1-y The thickness of the N quantum barrier layer is 10 nm.
[0086] The electron blocking layer 6 is a β-Ga₂O₃-graphene composite layer with a thickness of 90 nm. Specifically, the β-Ga₂O₃-graphene composite layer is prepared by annealing a β-Ga₂O₃ layer. After the β-Ga₂O₃ layer is grown, it is first kept at a temperature of 1150℃ and a pressure of 150 torr, and then annealed by introducing TMGa, SiH₄, and C₂H₄. The flow rate of TMGa is 70 sccm, the flow rate of SiH₄ is 30 sccm, and the flow rate of C₂H₄ is 150 sccm, with a purging time of 2 min. Then, annealing is carried out in an H₂ atmosphere at a temperature of 1600℃, a chamber pressure of 3 torr, and an annealing time of 20 min, thus obtaining the β-Ga₂O₃-graphene composite layer. Specifically, the thickness of the β-Ga₂O₃ layer is 120 nm.
[0087] Among them, the P-type semiconductor layer 7 is the first P-type β-Ga2O3-graphene composite layer with a thickness of 90 nm. The P-type dopant element is Mg, and the Mg doping concentration is 5 × 10⁻⁶. 20 cm -3 Specifically, the first p-type β-Ga₂O₃-graphene composite layer is obtained by annealing the first p-type β-Ga₂O₃ layer. Specifically, after the first p-type β-Ga₂O₃ layer is grown, it is first maintained at a temperature of 1150℃ and a pressure of 150 torr, and then annealed by introducing TMGa, SiH₄, and C₂H₄. The flow rate of TMGa is 70 sccm, the flow rate of SiH₄ is 30 sccm, and the flow rate of C₂H₄ is 150 sccm, with a purging time of 2 min. Then, annealing is performed in an H₂ atmosphere at a temperature of 1600℃, a chamber pressure of 3 torr, and an annealing time of 20 min, thus obtaining the first p-type β-Ga₂O₃-graphene composite layer. Specifically, the thickness of the first p-type β-Ga₂O₃ layer is 120 nm.
[0088] Among them, the P-type contact layer 8 is a second P-type β-Ga2O3-graphene composite layer with a thickness of 50 nm. The P-type dopant element is Mg, and the Mg doping concentration is 5 × 10⁻⁶. 21 cm -3Specifically, the second p-type β-Ga₂O₃-graphene composite layer is obtained by annealing the second p-type β-Ga₂O₃ layer. Specifically, after the second p-type β-Ga₂O₃ layer is grown, it is first maintained at 1150℃ and 150 torr, and then annealed by introducing TMGa, SiH₄, and C₂H₄. The flow rate of TMGa is 70 sccm, the flow rate of SiH₄ is 30 sccm, and the flow rate of C₂H₄ is 150 sccm, with a purging time of 2 min. Then, annealing is performed in an H₂ atmosphere at a temperature of 1600℃, a chamber pressure of 3 torr, and an annealing time of 20 min, thus obtaining the second p-type β-Ga₂O₃-graphene composite layer. Specifically, the thickness of the second p-type β-Ga₂O₃ layer is 60 nm.
[0089] The method for fabricating the epitaxial wafer of the ultraviolet light-emitting diode in this embodiment includes the following steps:
[0090] (1) Provide a substrate; load the substrate into MOCVD and anneal it at 1100℃, 400 torr, and hydrogen atmosphere for 6 min.
[0091] (2) Grow a buffer layer on the substrate;
[0092] Specifically, an AlN layer was grown using PVD as a buffer layer. The PVD equipment had a sputtering temperature of 500℃, a power of 4000W, and a pressure of 5 torr.
[0093] (3) An undoped AlGaN layer is grown on the buffer layer;
[0094] Specifically, undoped AlGaN layers were grown using MOCVD at a growth temperature of 1100℃ and a growth pressure of 70 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; H2 and N2 were used as carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.
[0095] (4) An N-type semiconductor layer is grown on an undoped AlGaN layer;
[0096] Specifically, an N-type semiconductor layer was grown using MOCVD at a growth temperature of 1150℃ and a growth pressure of 80 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source and SiH4 was introduced as an N-type doping source. H2 and N2 were used as carrier gases, TMGa was introduced as a Ga source, and TMAl was introduced as an Al source.
[0097] (5) Growing a multi-quantum-well layer on an N-type semiconductor layer;
[0098] Specifically, Al is periodically grown in MOCVD. x Ga 1-xN quantum well layer and Al y Ga 1-y An N-quantum barrier layer is used to obtain a multi-quantum-well layer. Al x Ga 1-x The growth temperature of the N quantum well layer was 950℃, and the growth pressure was 80 torr. Al y Ga 1-y The growth temperature of the N quantum barrier layer was 1050℃, and the growth pressure was 80 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, H2 and N2 were used as carrier gases, TEGa was introduced as the Ga source, and TMAl was introduced as the Al source.
[0099] (6) Growth of β-Ga2O3 layer on multi-quantum well layer;
[0100] The β-Ga2O3 layer was grown by MOCVD at a growth temperature of 1150℃ and a growth pressure of 150 torr. During growth, O2 was introduced as the O source and TMGa was introduced as the Ga source. The flow rate of O2 was 200 sccm and the flow rate of TMGa was 80 sccm.
[0101] (7) Anneal the β-Ga2O3 layer to obtain an electron blocking layer;
[0102] Specifically, the β-Ga2O3 layer is annealed in MOCVD to obtain the β-Ga2O3-graphene composite layer.
[0103] (8) A first p-type β-Ga2O3 layer is grown on the electron blocking layer;
[0104] Specifically, the first p-type β-Ga2O3 layer was grown in MOCVD at a growth temperature of 1150℃ and a growth pressure of 150 torr. During growth, O2 was introduced as the O source, TMGa as the Ga source, and Cp2Mg as the Mg source. The flow rate of O2 was 200 sccm, and the flow rate of TMGa was 80 sccm.
[0105] (9) Anneal the first P-type β-Ga2O3 layer to obtain a P-type semiconductor layer;
[0106] Specifically, the first P-type β-Ga2O3 layer is annealed in MOCVD to obtain the first P-type β-Ga2O3-graphene composite layer.
[0107] (10) A second P-type β-Ga2O3 layer is grown on the P-type semiconductor layer;
[0108] Specifically, a second p-type β-Ga2O3 layer was grown in MOCVD at a growth temperature of 1150℃ and a growth pressure of 150 torr. During growth, O2 was introduced as the O source, TMGa as the Ga source, and Cp2Mg as the Mg source. The flow rate of O2 was 200 sccm, and the flow rate of TMGa was 80 sccm.
[0109] (11) Anneal the second P-type β-Ga2O3 layer to obtain a P-type contact layer;
[0110] Specifically, the second P-type β-Ga2O3 layer is annealed in MOCVD to obtain the second P-type β-Ga2O3-graphene composite layer.
[0111] Example 2
[0112] This embodiment provides an epitaxial wafer for an ultraviolet light-emitting diode, which differs from Embodiment 1 in that the Mg doping concentration in the first P-type β-Ga2O3-graphene composite layer is 5 × 10⁻⁶. 19 cm -3 The Mg doping concentration in the second p-type β-Ga2O3-graphene composite layer is 5 × 10⁻⁶. 20 cm -3 .
[0113] Everything else is the same as in Example 1.
[0114] Example 3
[0115] This embodiment provides an epitaxial wafer for an ultraviolet light-emitting diode, which differs from Embodiment 2 in that the thickness of the β-Ga2O3-graphene composite layer is 40 nm, the thickness of the first P-type β-Ga2O3-graphene composite layer is 40 nm, and the thickness of the second P-type β-Ga2O3-graphene composite layer is 20 nm.
[0116] Everything else is the same as in Example 2.
[0117] Comparative Example 1
[0118] This comparative example provides an epitaxial wafer for an ultraviolet light-emitting diode, which differs from Example 1 in that the electron blocking layer 6 is Al. γ Ga 1-γ The N-layer (γ = 0.6) has a thickness of 90 nm; the P-type semiconductor layer 7 is a P-type AlGaN layer, with Mg as the P-type dopant and a Mg doping concentration of 5 × 10⁻⁶. 20 cm -3 Its thickness is 90 nm; the P-type contact layer 8 is a Mg-doped AlGaN layer with a Mg doping concentration of 5 × 10⁻⁶. 21 cm -3Its thickness is 50 nm. Correspondingly, in the preparation method, Al is grown using MOCVD. γ Ga 1-γ The N-layer serves as an electron blocking layer. The growth temperature is 1050℃ and the growth pressure is 200 torr. The P-type AlGaN layer is grown using MOCVD at the same temperature and pressure. The P-type contact layer is also grown using MOCVD at the same temperature and pressure.
[0119] Everything else is the same as in Example 1.
[0120] The brightness and operating voltage of the LED epitaxial wafers obtained in Examples 1-3 and Comparative Example 1 were tested. The specific test methods are as follows:
[0121] (1) The epitaxial wafer was fabricated into a chip with a size of 20mil×20mil, and its luminous brightness was tested under a current of 40mA;
[0122] (2) Use a Keithley 2450 digital source meter to test the operating voltage.
[0123] The specific results are as follows:
[0124] Brightness (mW) Operating voltage (V) Example 1 5.178 6.10 Example 2 5.329 6.08 Example 3 5.516 6.07 Comparative Example 1 4.464 6.17
[0125] As can be seen from the table, when the traditional structure of the light-emitting diode electron blocking layer, P-type semiconductor layer, and P-type contact layer (Comparative Example 1) is used, the brightness is increased to 5.178mW and the operating voltage is reduced to 6.10V, indicating that the present invention can effectively improve brightness and reduce operating voltage. Furthermore, a comparison between Example 1 and Comparative Examples 2-3 shows that changing the structure in the present invention is unlikely to effectively improve brightness and reduce operating voltage.
[0126] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. An epitaxial wafer for an ultraviolet light-emitting diode, comprising a substrate and a buffer layer, an undoped AlGaN layer, an N-type semiconductor layer, a multiple quantum well layer, an electron blocking layer, a P-type semiconductor layer, and a P-type contact layer sequentially disposed on the substrate; characterized in that, The electron blocking layer is a β-Ga2O3-graphene composite layer, the P-type semiconductor layer is a first P-type β-Ga2O3-graphene composite layer, and the P-type contact layer is a second P-type β-Ga2O3-graphene composite layer. The thickness of the β-Ga2O3-graphene composite layer is 10nm-80nm; The p-type dopant element in the first p-type β-Ga2O3-graphene composite layer is Mg, and the Mg doping concentration is 1×10⁻⁶. 19 cm -3 -1×10 20 cm -3 The thickness of the first P-type β-Ga2O3-graphene composite layer is 20nm-80nm; The second p-type β-Ga2O3-graphene composite layer has Mg as the p-type dopant, and the Mg doping concentration is 1×10⁻⁶. 20 cm -3 -1×10 21 cm -3 The thickness of the second P-type β-Ga2O3-graphene composite layer is 5nm-40nm.
2. The ultraviolet light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the second P-type β-Ga2O3-graphene composite layer is less than the thickness of the first P-type β-Ga2O3-graphene composite layer.
3. The ultraviolet light-emitting diode epitaxial wafer as described in claim 1 or 2, characterized in that, The β-Ga2O3-graphene composite layer is obtained by annealing a β-Ga2O3 layer; The first P-type β-Ga2O3-graphene composite layer is obtained by annealing the first P-type β-Ga2O3 layer; The second P-type β-Ga2O3-graphene composite layer is obtained by annealing the second P-type β-Ga2O3 layer.
4. The ultraviolet light-emitting diode epitaxial wafer as described in claim 3, characterized in that, After the β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. Then, TMGa, SiH4, and C2H4 are introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm, with an introduction time of 1 min-3 min. Next, annealing is performed in an H2 atmosphere at a temperature of 1500℃-1700℃, an annealing chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min. This yields the β-Ga2O3-graphene composite layer. After the first P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm. The introduction time is 1 min-3 min. Annealing is then performed in an H2 atmosphere at a temperature of 1500℃-1700℃, a chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min. This yields the first P-type β-Ga2O3-graphene composite layer. After the second P-type β-Ga2O3 layer is grown, the temperature is maintained at 1100℃-1200℃ and the pressure at 100 torr-200 torr. TMGa, SiH4, and C2H4 are then introduced for annealing. The flow rate of TMGa is 50 sccm-100 sccm, the flow rate of SiH4 is 10 sccm-50 sccm, and the flow rate of C2H4 is 100 sccm-200 sccm. The introduction time is 1 min-3 min. Annealing is then performed in an H2 atmosphere at a temperature of 1500℃-1700℃, a chamber pressure of 0 torr-5 torr, and an annealing time of 10 min-30 min. This yields the second P-type β-Ga2O3-graphene composite layer.
5. The ultraviolet light-emitting diode epitaxial wafer as described in claim 3, characterized in that, The thickness of the β-Ga2O3 layer is 20nm-100nm; The thickness of the first P-type β-Ga2O3 layer is 30nm-100nm; The thickness of the second P-type β-Ga2O3 layer is 10nm-50nm.
6. A method for preparing an ultraviolet light-emitting diode epitaxial wafer, used to prepare the ultraviolet light-emitting diode epitaxial wafer as described in any one of claims 1-5, characterized in that, include: A substrate is provided on which a buffer layer, an undoped AlGaN layer, an N-type semiconductor layer, a multiple quantum well layer, an electron blocking layer, a P-type semiconductor layer, and a P-type contact layer are sequentially grown; the electron blocking layer is a β-Ga2O3-graphene composite layer, the P-type semiconductor layer is a first P-type β-Ga2O3-graphene composite layer, and the P-type contact layer is a second P-type β-Ga2O3-graphene composite layer. The thickness of the β-Ga2O3-graphene composite layer is 10nm-80nm; The p-type dopant element in the first p-type β-Ga2O3-graphene composite layer is Mg, and the Mg doping concentration is 1×10⁻⁶. 19 cm -3 -1×10 20 cm -3 The thickness of the first P-type β-Ga2O3-graphene composite layer is 20nm-80nm; The second p-type β-Ga2O3-graphene composite layer has Mg as the p-type dopant, and the Mg doping concentration is 1×10⁻⁶. 20 cm -3 -1×10 21 cm -3 The thickness of the second P-type β-Ga2O3-graphene composite layer is 5nm-40nm.
7. The method for fabricating an ultraviolet light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The β-Ga2O3-graphene composite layer is obtained by annealing the β-Ga2O3 layer. The growth temperature of the β-Ga2O3 layer is 1100℃-1200℃, the growth pressure is 100 torr-200 torr, and during growth, O2 is introduced as the O source and TMGa is introduced as the Ga source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm. The first P-type β-Ga2O3-graphene composite layer is obtained by annealing the first P-type β-Ga2O3 layer. The growth temperature of the first P-type β-Ga2O3 layer is 1100℃-1200℃, the growth pressure is 100 torr-200 torr, and during growth, O2 is introduced as the O source, TMGa is introduced as the Ga source, and Cp2Mg is introduced as the Mg source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm. The second P-type β-Ga2O3-graphene composite layer is obtained by annealing the second P-type β-Ga2O3 layer. The growth temperature of the second P-type β-Ga2O3 layer is 1100℃-1200℃, and the growth pressure is 100 torr-200 torr. During growth, O2 is introduced as the O source, TMGa is introduced as the Ga source, and Cp2Mg is introduced as the Mg source. The flow rate of O2 is 100 sccm-300 sccm, and the flow rate of TMGa is 50 sccm-100 sccm.
8. A light-emitting diode, characterized in that, Includes the ultraviolet light-emitting diode epitaxial wafer as described in any one of claims 1-5.
Citation Information
Patent Citations
Light-emitting diode
CN103137811A
Light-emitting diode chip manufacturing method and light-emitting diode chip
JP2018029110A