A nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, a preparation method thereof and a lithium-sulfur battery

By preparing nitrogen-doped carbon polyhedral materials embedded with MoC/WC quantum dots, the problem of easy agglomeration of transition metal carbide nanoparticles was solved, thereby improving the performance and enabling large-scale production of lithium-sulfur batteries.

CN117650337BActive Publication Date: 2026-11-20SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311439332.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-31
Publication Date
2026-11-20
Estimated Expiration
2043-10-31

AI Technical Summary

Technical Problem

In existing technologies, transition metal carbide nanoparticles are prone to agglomeration, making it difficult to control the synthesis and size uniformity of nanoscale products, resulting in limited performance improvements in lithium-sulfur batteries.

Method used

HZIF-ZnMoW material was prepared by reacting zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone and dimethylimidazole in N,N-dimethylformamide. After annealing, a nitrogen-doped carbon polyhedral material with MoC/WC quantum dots was formed. This material was then used to modify lithium-sulfur battery separators. Graphite sheet coating was used to prevent agglomeration and maintain dimensional uniformity.

Benefits of technology

Effective control of the size uniformity of MoC/WC quantum dots improves the charge-discharge specific capacity of lithium-sulfur batteries, reduces the capacity decay rate during the reaction process, and exhibits excellent electrochemical performance, making them suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117650337B_ABST
    Figure CN117650337B_ABST
Patent Text Reader

Abstract

The application discloses a kind of nitrogen-doped carbon polyhedral materials embedded with MoC / WC quantum dots and a kind of lithium-sulfur battery, and the preparation method of the nitrogen-doped carbon polyhedral materials includes zinc acetate, molybdate, tungstate, polyvinylpyrrolidone and dimethylimidazole are added in N, N-dimethylformamide, after being fully stirred to completely dissolved, HZIF-ZnMoW is prepared;The nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is prepared after HZIF-ZnMoW is annealed.The preparation method is safe and simple, and the preparation period is short, and the required equipment is simple, the size of MoC quantum dot and WC quantum dot prepared is 2-5 nanometers, and MoC / WC quantum dot outer layer is covered by graphite sheet layer, with good conductivity, adsorption performance and catalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of lithium-sulfur battery separator modification materials, and relates to a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, its preparation method, and a lithium-sulfur battery. Background Technology

[0002] Electrochemical energy storage devices store electrical energy in the form of chemical energy and release it as electrical energy when needed, making them a very suitable energy storage system. Lithium-sulfur batteries, composed of a sulfur cathode and a lithium metal anode, have an extremely high theoretical specific capacity (1675 mAh g⁻¹). -1 ) and theoretical specific energy (2600Wh kg) -1 Lithium-sulfur batteries are attracting widespread attention globally. Importantly, the natural abundance and low cost of sulfur ensure that lithium-sulfur batteries are an environmentally friendly and high-potential energy storage device. Furthermore, lithium metal's advantages of light weight and low standard potential also make it a promising energy system. Sulfur and polysulfides (Li₂S₂) x Li₂S is electrically insulating. x Polysulfides may dissolve in liquid electrolytes, and their volume may change during the conversion reaction. During charge and discharge, soluble polysulfides at the cathode may react with lithium metal at the anode through the separator to form insoluble Li2S and Li2S2, resulting in a "shuttle effect" that leads to short battery cycle life, low sulfur utilization, low efficiency, and rapid capacity decay.

[0003] To address the above issues, the most effective methods can be categorized into improvements to three key components of lithium-sulfur batteries: the cathode, the separator, and the functional layer. This includes the construction of the sulfur cathode substrate, the modification of the separator, the fabrication of the functional layer between the cathode and the separator, and the regulation of the electrolyte system. Among these, modifying the separator to capture and restrict polysulfide shuttle is an effective method for optimizing battery performance. Transition metal carbides, due to their excellent electrochemical activity, high conductivity, and chemical stability, have been used for separator modification. However, the tendency of nanoparticles to aggregate makes it difficult to control the synthesis of nanoscale products, and the size uniformity of nanoparticles cannot be effectively controlled, resulting in limited improvements in battery performance. Summary of the Invention

[0004] To address the problems existing in the prior art, this invention provides a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, its preparation method, and a lithium-sulfur battery. This solves the technical problem that in the preparation of transition metal carbides, it is difficult to control the synthesis of nanoscale products due to the aggregation of nanoparticles, and at the same time, it is impossible to effectively control the size uniformity of nanoparticles, resulting in limited improvement of battery performance.

[0005] This invention is achieved through the following technical solution:

[0006] A method for preparing a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots includes the following steps:

[0007] S1: Zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone and dimethylimidazole are added to N,N-dimethylformamide and stirred thoroughly until completely dissolved to prepare HZIF-ZnMoW;

[0008] S2: The nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is obtained by annealing the HZIF-ZnMoW.

[0009] Preferably, in step S1, the mass ratio of zinc acetate to molybdic acid and tungstic acid is (3-6):(0.5-1):(0.5-1).

[0010] Preferably, in step S1, the mass ratio of zinc acetate to dimethylimidazole is (3-6):(2-5).

[0011] Preferably, in step S1, the stirring temperature is 80℃~200℃ and the stirring time is 6~12h.

[0012] Preferably, before step S2, the prepared HZIF-ZnMoW is further subjected to a drying process, wherein the drying temperature is 60℃~100℃ and the drying time is 6~12h.

[0013] Preferably, in step S2, during the annealing process, the annealing temperature is 500℃~1200℃ and the annealing time is 0.5~6h.

[0014] A nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is prepared by the method described in any one of claims 1 to 6.

[0015] A lithium-sulfur battery separator, fabricated from the aforementioned nitrogen-doped polyhedral material embedded with MoC / WC quantum dots, comprises the following steps:

[0016] S11: Add the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots into PVDF, stir and mix evenly to obtain a membrane modification solution;

[0017] S12: The membrane modification liquid is uniformly coated on the PP membrane to obtain the lithium-sulfur battery membrane.

[0018] Preferably, in step S11, the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is (6-9):(4-1).

[0019] A lithium-sulfur battery comprising the aforementioned lithium-sulfur battery separator, wherein the lithium-sulfur battery has a discharge specific capacity of 550-700 mAh / g after 1000 cycles at a current density of 1C.

[0020] Compared with the prior art, the present invention has the following beneficial technical effects:

[0021] This invention discloses a method for preparing a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots. First, zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone, and dimethylimidazole are added to N,N-dimethylformamide and stirred thoroughly until completely dissolved to obtain HZIF-ZnMoW. This material is an HZIF framework material with Zn, Mo, and W ions on the metal sites. Then, the material is annealed. After annealing, Mo and W ions are reduced to MoC and WC quantum dots, respectively, while Zn ions are vaporized. The HZIF framework forms a nitrogen-doped carbon polyhedral carbon skeleton. Simultaneously, the catalytic properties of the MoC and WC quantum dots themselves cause the HZIF framework material to form graphitized carbon during carbonization, which coats the surfaces of the MoC and WC quantum dots, effectively preventing their aggregation. The resulting graphite-coated MoC and WC quantum dots are embedded in the nitrogen-doped carbon polyhedral carbon skeleton. This method effectively controls the size of MoC and WC quantum dots, ensuring the size uniformity of the product. Simultaneously, using HZIF as a self-template, the original morphology can be maintained after high-temperature annealing, resulting in high mechanical strength and maintaining the high porosity of the HZIF material. Due to the embedded uniform MoC / WC quantum dots, this material exhibits good catalytic conversion ability. When used as a separator modifier for lithium-sulfur batteries, it effectively promotes the catalytic conversion of polysulfides and improves the shuttle effect of lithium-sulfur batteries, increasing the charge-discharge specific capacity and reducing the capacity decay rate during the reaction process. It possesses excellent electrochemical performance and is suitable for large-scale production. This preparation method is safe and simple, with a short preparation cycle and simple equipment requirements. The prepared quantum dots have uniform size and are coated with graphite sheets, which effectively prevent the quantum dots from agglomerating into larger particles. Furthermore, the graphite sheets possess good electrical conductivity, adsorption properties, and catalytic performance.

[0022] Furthermore, the mass ratio of zinc acetate to molybdic acid and tungstic acid is (3-6):(0.5-1):(0.5-1), which can sufficiently allow metal ions to be doped into the HZIF framework structure.

[0023] Furthermore, the mass ratio of zinc acetate to dimethylimidazole is (3-6):(2-5), which can fully ensure the synthesis of HZIF-ZnMoW.

[0024] Furthermore, in step S1, the stirring temperature is 80℃~200℃ and the stirring time is 6~12h, which allows zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone and dimethylimidazole to be fully dissolved, resulting in a homogeneous system and ensuring the homogeneity of the product.

[0025] Furthermore, before step S2, the prepared HZIF-ZnMoW is dried. During the drying process, the drying temperature is 60℃~100℃ and the drying time is 6~12h. This process can fully remove the moisture from the material and avoid the influence on the chemical composition and physical structure of the product during the subsequent annealing process, thus ensuring the purity and size uniformity of the product.

[0026] Furthermore, in step S2, during the annealing process, the annealing temperature is 500℃~1200℃ and the annealing time is 0.5~6h. These annealing conditions allow the HZIF framework material to be fully carbonized and the zinc to be fully vaporized. At the same time, the molybdenum ions and tungsten ions are reduced to carbides to obtain MoC / WC quantum dots with uniform size. Meanwhile, after the HZIF framework material is carbonized, some of it forms graphite sheets that wrap around the outer layer of the MoC / WC quantum dots.

[0027] Meanwhile, the present invention also discloses a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots obtained by the above method.

[0028] Furthermore, this invention also discloses a lithium-sulfur battery separator prepared from a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots obtained by the above method. The lithium-sulfur battery separator is prepared by first adding the MoC / WC quantum dot-embedded nitrogen-doped carbon polyhedral material to PVDF, and then coating it onto a PP separator. The preparation method is simple, the design is reasonable, and it is easy to scale up for development and application.

[0029] Furthermore, the mass ratio of the nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots to PVDF is (6-9):(4-1), which effectively allows the nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots to adhere to the PP substrate film. At the same time, after drying, the nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots will not be encapsulated by PVDF, ensuring the performance of the nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots. If the PVDF content is too low, the adhesion of the nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots to the PP substrate film will not be strong, resulting in a decrease in battery performance.

[0030] Meanwhile, the present invention also discloses a lithium-sulfur battery comprising the above-mentioned lithium-sulfur battery separator, which has a discharge specific capacity of 550-700 mAh / g after 1000 cycles at a current density of 1C, and has excellent electrical performance. Attached Figure Description

[0031] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0032] Figure 1 This is a schematic flowchart of a method for preparing a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots according to the present invention.

[0033] Figure 2 The images show SEM characterization images of the nitrogen-doped carbon polyhedral material with MoC / WC quantum dots embedded in it, prepared in Example 1 of this invention, before and after annealing. The left image is before annealing, and the right image is after annealing.

[0034] Figure 3 The images show TEM images of the nitrogen-doped carbon polyhedral material with MoC / WC quantum dots embedded in it, prepared in Example 1 of this invention, before and after annealing. The left image is before annealing, and the right image is after annealing.

[0035] Figure 4 The image shows the XRD pattern of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots obtained in Example 1 of this invention.

[0036] Figure 5 The image shows the charge-discharge curves of a lithium-sulfur battery prepared using the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots obtained in Example 1 of this invention. Detailed Implementation

[0037] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0038] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0039] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0040] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0041] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0042] like Figure 1 As shown, this invention provides a method for preparing a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, comprising the following steps:

[0043] S1: Zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone, and dimethylimidazole are added to N,N-dimethylformamide and stirred at 80℃~200℃ for 6~12h until completely dissolved to obtain HZIF-ZnMoW. The obtained HZIF-ZnMoW is dried at 60℃~100℃ for 6~12h to obtain dried HZIF-ZnMoW.

[0044] The mass ratio of zinc acetate to molybdic acid and tungstic acid is (3-6):(0.5-1):(0.5-1).

[0045] The mass ratio of zinc acetate to dimethylimidazole is (3-6):(2-5).

[0046] S2: Anneal the dried HZIF-ZnMoW to obtain the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots.

[0047] During the annealing process, the annealing temperature is 500℃~1200℃ and the annealing time is 0.5~6h.

[0048] This invention also discloses a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, prepared by the above method. The size of the MoC and WC quantum dots is 2–5 nanometers; furthermore, both the MoC and WC quantum dots are coated with 3–6 layers of graphite sheets, which effectively prevent the quantum dots from agglomerating into larger particles. The graphite-coated MoC and WC quantum dots are embedded within a nitrogen-doped carbon polyhedral carbon framework.

[0049] In addition, the present invention also discloses a lithium-sulfur battery separator, which is prepared by the above-mentioned nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots, and includes the following steps:

[0050] A lithium-sulfur battery separator, characterized in that it is prepared by using a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots as described in claim 7, comprising the following steps:

[0051] S11: Add the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF, stir and mix evenly to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is (6~9):(4~1);

[0052] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0053] S13: Dry the PP diaphragm coated with the modified liquid at 40℃~80℃ for 6~12h.

[0054] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0055] In addition, the present invention also discloses a lithium-sulfur battery separator comprising the above-mentioned lithium-sulfur battery, wherein the lithium-sulfur battery has a discharge specific capacity of 550-700 mAh / g after 1000 cycles at a current density of 1C.

[0056] This invention discloses a method for preparing a nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots. First, zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone, and dimethylimidazole are added to N,N-dimethylformamide and stirred thoroughly until completely dissolved to obtain HZIF-ZnMoW. This material is an HZIF framework material with Zn, Mo, and W ions disposed on metal sites. Then, the material is annealed. After annealing, Mo and W ions are reduced to MoC and WC quantum dots, respectively, while Zn ions are vaporized. The HZIF framework forms a nitrogen-doped carbon polyhedral carbon skeleton, with the MoC and WC quantum dots embedded in the nitrogen. In a carbon-doped polyhedral carbon framework, this method effectively controls the size of MoC and WC quantum dots to 2–5 nanometers, ensuring the size uniformity of the product. Simultaneously, using HZIF as a self-template, the original morphology can be maintained after high-temperature annealing, resulting in high mechanical strength and maintaining the high porosity of the HZIF material. Due to the embedded uniform MoC / WC quantum dots, this material exhibits high ionic conductivity. Using it as a separator modifier for lithium-sulfur batteries effectively improves the shuttle effect, increases the charge / discharge specific capacity, reduces the capacity decay rate during the reaction process, and demonstrates excellent electrochemical performance, making it suitable for large-scale production. This preparation method is safe and simple, with a short preparation cycle and simple equipment requirements. The prepared product has uniform size and a uniformly coated graphene layer, exhibiting good electrical conductivity, adsorption properties, and catalytic performance.

[0057] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0058] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0059] Example 1

[0060] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. The raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 3:0.5:0.5, and the mass ratio of zinc acetate to dimethylimidazole was 3:2. The mixture was stirred at 160℃ for 5 hours. After complete dissolution, a white powder, HZIF-ZnMoW, was filtered and dried at 60℃ for 5 hours. After drying, the mixture was annealed at 1200℃ for 0.5 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC quantum dots and WC quantum dots.

[0061] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0062] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 6:4.

[0063] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0064] S13: Dry the PP diaphragm coated with the modified liquid at 40°C for 6 hours;

[0065] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0066] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 700 mAh / g after 1000 cycles at a current density of 1C.

[0067] Example 2

[0068] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. The raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 3.5:1:1, and the mass ratio of zinc acetate to dimethylimidazole was 4:3. The mixture was stirred at 150°C for 6 hours. After complete dissolution, a white powder, HZIF-ZnMoW, was filtered and dried at 70°C for 6 hours. After drying, the mixture was annealed and held at 1100°C for 1 hour to form a nitrogen-doped carbon polyhedral material embedded with MoC quantum dots and WC quantum dots.

[0069] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0070] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred to mix evenly to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 7:3.

[0071] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0072] S13: Dry the PP diaphragm coated with the modified liquid at 50°C for 7 hours.

[0073] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0074] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 680 mAh / g after 1000 cycles at a current density of 1C.

[0075] Example 3

[0076] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. These raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 4:1:1, and the mass ratio of zinc acetate to dimethylimidazole was 5:3. The mixture was stirred at 160℃ for 7 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 80℃ for 7 hours. After drying, annealing was performed at 1000℃ for 2 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0077] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0078] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 8:2.

[0079] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0080] S13: Dry the PP diaphragm coated with the modified liquid at 60°C for 8 hours;

[0081] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0082] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 660 mAh / g after 1000 cycles at a current density of 1C.

[0083] Example 4

[0084] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. These raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 5:1:1, and the mass ratio of zinc acetate to dimethylimidazole was 6:4. The mixture was stirred at 170℃ for 8 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 90℃ for 8 hours. After drying, annealing was performed at 900℃ for 3 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0085] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0086] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 9:1.

[0087] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0088] S13: Dry the PP diaphragm coated with the modified liquid at 70°C for 9 hours;

[0089] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0090] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 640 mAh / g after 1000 cycles at a current density of 1C.

[0091] Example 5

[0092] Using zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid as raw materials, the raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 5:0.5:0.5, and the mass ratio of zinc acetate to dimethylimidazole was 6:5. The mixture was stirred at 180℃ for 9 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 100℃ for 9 hours. After drying, it underwent annealing at 800℃ for 4 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0093] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0094] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 9:2.

[0095] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0096] S13: Dry the PP diaphragm coated with the modified liquid at 80°C for 10 hours.

[0097] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0098] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 620 mAh / g after 1000 cycles at a current density of 1C.

[0099] Example 6

[0100] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. These raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 4:0.5:0.5, and the mass ratio of zinc acetate to dimethylimidazole was 6:4. The mixture was stirred at 110℃ for 10 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 110℃ for 10 hours. After drying, annealing was performed at 700℃ for 5 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0101] The lithium-sulfur battery separator was prepared using this nitrogen-doped multi-carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0102] S11: Nitrogen-doped polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 9:3.

[0103] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0104] S13: Dry the PP diaphragm coated with the modified liquid at 40°C for 10 hours.

[0105] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0106] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 600 mAh / g after 1000 cycles at a current density of 1C.

[0107] Example 7

[0108] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. These raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 3:0.5:0.5, and the mass ratio of zinc acetate to dimethylimidazole was 3:5. The mixture was stirred at 100℃ for 11 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 120℃ for 11 hours. After drying, annealing was performed at 700℃ for 5 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0109] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0110] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 9:4.

[0111] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0112] S13: Dry the PP diaphragm coated with the modified liquid at 50°C for 10 hours.

[0113] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0114] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 580 mAh / g after 1000 cycles at a current density of 1C.

[0115] Example 8

[0116] Zinc acetate (Zn(CH3COO)·2H2O), molybdic acid, and tungstic acid were used as raw materials. These raw materials, along with polyvinylpyrrolidone (PVP(K30)) and dimethylimidazole, were added to N,N-dimethylformamide (DMF). The mass ratio of zinc acetate to molybdic acid and tungstic acid was 4:1:1, and the mass ratio of zinc acetate to dimethylimidazole was 4:5. The mixture was stirred at 90℃ for 12 hours until completely dissolved. The resulting white powder, HZIF-ZnMoW, was filtered and dried at 130℃ for 12 hours. After drying, it underwent annealing at 600℃ for 6 hours to form a nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots.

[0117] The lithium-sulfur battery separator was prepared using this nitrogen-doped carbon polyhedral material embedded with MoC and WC quantum dots. The specific preparation process is as follows:

[0118] S11: Nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots is added to PVDF and stirred until homogeneous to obtain a membrane modification solution; the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is 7:4.

[0119] S12: The membrane modification liquid is evenly coated onto the PP membrane using a scraper;

[0120] S13: Dry the PP diaphragm coated with the modified liquid at 50°C for 12 hours.

[0121] S14: Cut the dried separator into round pieces with a diameter of 12mm to obtain the lithium-sulfur battery separator.

[0122] Furthermore, a lithium-sulfur battery separator was prepared using this lithium-sulfur battery separator. The lithium-sulfur battery obtained in this embodiment has a discharge specific capacity of 550 mAh / g after 1000 cycles at a current density of 1C.

[0123] Since the nitrogen-doped carbon polyhedral materials with MoC / WC quantum dots prepared in the above embodiments have basically the same structure and properties, the following description will only focus on the structure and properties of the nitrogen-doped carbon polyhedral materials with MoC / WC quantum dots obtained by modification in Example 1.

[0124] SEM characterization of nitrogen-doped carbon polyhedral materials embedded with MoC / WC quantum dots before and after annealing was performed, and the results are as follows: Figure 2 As shown. By Figure 2 It can be seen that the material retains the original HZIF morphology after annealing, indicating that the material has good mechanical strength. At the same time, a porous structure is formed on the surface, which can adsorb and accommodate more polysulfides, thus improving the performance of the lithium-sulfur battery separator.

[0125] TEM characterization of nitrogen-doped carbon polyhedral materials embedded with MoC / WC quantum dots before and after annealing was performed. Figure 3 It is known that ultrafine MoC / WC quantum dots are generated therein, with a size of about 2 to 5 nanometers, and the outer layer of the quantum dots is covered by 3 to 6 layers of graphene. These ultrafine MoC / WC quantum dots can better catalyze the conversion of long-chain polysulfides that are dissolved in the electrolyte into short-chain polysulfides, effectively improving the performance of the battery.

[0126] XRD characterization of nitrogen-doped carbon polyhedral materials embedded with MoC / WC quantum dots was performed, and the results are as follows: Figure 4 As shown. By Figure 4 It can be seen that the annealing treatment produced obvious diffraction peaks of WC and MoC, indicating that MoC quantum dots and WC quantum dots exist in the carbon framework of HZIF.

[0127] The obtained materials were characterized for electrochemical performance. A lithium-sulfur battery separator was prepared using the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots obtained in Example 1. A lithium-sulfur battery was then assembled using this separator, and the charge-discharge performance of the lithium-sulfur battery was tested. Specific test results are shown below. Figure 5 ,Depend on Figure 5 It can be seen that within the voltage range of 1.7 to 2.8V, at a 1C rate, the capacity can still reach 600mAh g after 1000 cycles. -1 .

[0128] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A lithium-sulfur battery separator, characterized in that, It was prepared from nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots; The preparation of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots includes the following steps: S1: Zinc acetate, molybdic acid, tungstic acid, polyvinylpyrrolidone and dimethylimidazole are added to N,N-dimethylformamide and stirred thoroughly until completely dissolved to prepare HZIF-ZnMoW; S2: The nitrogen-doped carbon polyhedron material embedded with MoC / WC quantum dots is obtained by annealing the HZIF-ZnMoW. The preparation of the lithium-sulfur battery separator includes the following steps: S11: Add the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots into PVDF, stir and mix evenly to obtain a membrane modification solution; S12: The membrane modification liquid is uniformly coated on the PP membrane to obtain the lithium-sulfur battery membrane.

2. The lithium-sulfur battery separator according to claim 1, characterized in that, In step S1, the mass ratio of zinc acetate to molybdic acid and tungstic acid is (3~6):(0.5~1):(0.5~1).

3. The lithium-sulfur battery separator according to claim 1, characterized in that, In step S1, the mass ratio of zinc acetate to dimethylimidazole is (3~6):(2~5).

4. A lithium-sulfur battery separator according to claim 1, characterized in that, In step S1, the stirring temperature is 80℃~200℃, and the stirring time is 6~12h.

5. A lithium-sulfur battery separator according to claim 1, characterized in that, Before step S2, the prepared HZIF-ZnMoW is dried. During the drying process, the drying temperature is 60℃~100℃ and the drying time is 6~12h.

6. A lithium-sulfur battery separator according to claim 1, characterized in that, In step S2, during the annealing process, the annealing temperature is 500℃~1200℃ and the annealing time is 0.5~6h.

7. A lithium-sulfur battery separator according to claim 1, characterized in that, In step S11, the mass ratio of the nitrogen-doped carbon polyhedral material embedded with MoC / WC quantum dots to PVDF is (6~9):(4~1).

8. A lithium-sulfur battery, characterized in that, The lithium-sulfur battery includes a separator according to any one of claims 1 to 7, wherein the lithium-sulfur battery has a discharge specific capacity of 550 to 700 mAh / g after 1000 cycles at a current density of 1C.

Citation Information

Patent Citations

  • Lithium-sulfur battery positive plate and preparation method thereof, and lithium-sulfur battery

    CN109786748A

  • Nitrogen-doped MoxC / Co / carbon nanotube composite material and preparation method and application thereof

    CN114300668A