Polyimide coverings

By combining diamine monomers and dianhydride monomers with specific structures and silane compounds, polyimide coatings were prepared, solving the problems of partial discharge and insufficient flexibility of polyimide resins under high voltage. This resulted in low dielectric constant, high dielectric breakdown voltage, and excellent adhesion and flexibility, thereby improving the reliability of electrical equipment.

CN117651739BActive Publication Date: 2026-11-20PI ADVANCED MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280050450.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-20
Filing Date
2022-07-20
Publication Date
2026-11-20
Estimated Expiration
2042-07-20

AI Technical Summary

Technical Problem

Existing polyimide resins are prone to partial discharge and insulation breakdown when used under high voltage, and their insufficient flexibility affects the lifespan and reliability of electrical equipment.

Method used

Polyimide coatings are prepared using diamine monomers and dianhydride monomers with specific structures. Combined with silane compounds, they ensure low dielectric constant, excellent adhesion and flexibility. By adjusting the ratio and content of diamine monomers and dianhydride monomers, the dielectric breakdown voltage and mechanical properties are improved.

Benefits of technology

It achieves low dielectric constant and high dielectric breakdown voltage in the high frequency range, enhances the adhesion between the conductor and the covering and the flexibility of the covering, prevents partial discharge and insulation breakdown, and improves the reliability of electrical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_5
    Figure QLYQS_5
  • Figure BDA0004668473970000031
    Figure BDA0004668473970000031
Patent Text Reader

Abstract

The present invention provides a covering, which is a polyimide covering, and has low dielectric properties and prevents insulation breakdown and partial discharge, while improving adhesion between the conductor and the covering and flexibility of the covering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a polyimide coating. Background Technology

[0002] The insulating layer (coating) covering the conductor needs to have excellent insulation, adhesion to the conductor, heat resistance, or mechanical strength, etc.

[0003] Furthermore, in electrical devices with high applied voltages, such as motors used under high voltage, high voltage is applied to the insulated wires constituting the electrical device, thereby making it easy for partial discharge (corona discharge) to occur on their coating surface.

[0004] Because corona discharge can cause local temperature increases or generate ozone or ions, it can lead to deterioration of the insulation coating of wires, resulting in premature insulation breakdown and shortening the life of electrical equipment.

[0005] For the reasons mentioned above, insulated wires used under high voltage require a higher corona discharge initiation voltage, and it is known that reducing the dielectric constant of the insulation layer is effective for this purpose.

[0006] The resin that forms the insulating layer includes polyimide resin, polyamide-imide resin, or polyester-imide resin, etc.

[0007] Generally speaking, polyimide resin refers to a high heat-resistant resin prepared by solution polymerization of aromatic dianhydrides and aromatic diamines or aromatic diisocyanates to prepare polyamic acid derivatives, followed by ring-closure dehydration and imidization at high temperature.

[0008] Polyimide resin is a material with excellent heat resistance and relatively low dielectric constant, making it ideal for use as a conductor coating material.

[0009] On the other hand, because polyimide resin has a rigid structure, it has low elongation at break and low flexibility, which makes it unsuitable for use as a cover for conductors.

[0010] For example, in the coils used in motors, in order to increase the duty cycle, a process that significantly deforms the insulated wire can be performed, such as winding the insulated wire into a coil and then inserting the coil into a slot, etc.

[0011] If the insulation layer has low flexibility, there is a possibility that the covering may be damaged or cracked during processing.

[0012] To improve flexibility, when polyimide resins are prepared by reacting diamines and dianhydrides with flexible structures, there is a problem of reduced heat resistance compared to polyimide resins that do not contain diamines or dianhydrides with flexible structures.

[0013] Therefore, there is a need to develop a technology that can improve corona resistance while maintaining the adhesion between the conductor and the cover, as well as the flexibility of the cover. Summary of the Invention

[0014] Technical issues

[0015] The purpose of this invention is to solve the problems and technical challenges of the prior art. This application provides a polyimide coating that has a low dielectric constant, which can prevent dielectric breakdown and partial discharge, while improving the adhesion between the conductor and the coating and the flexibility of the coating.

[0016] Solution to the problem

[0017] This application relates to a polyimide. The polyimide described above can be applied to conductive coatings. This application provides a polyimide coating. The polyimide coating described above may comprise a polyimide having dianhydride monomer components and diamine monomer components as polymerization units.

[0018] The polyimide coating according to this application has a dielectric constant Dk of less than 3.6 in the 10 GHz band. There is no particular limitation on the lower limit of the cured dielectric constant; for example, it can be above 1.0, and the upper limit can be below 3.58, 3.55, 3.53, 3.5, 3.48, 3.45, or 3.42. The polyimide resin cured from the polyamic acid composition of this application has a low dielectric constant, especially in the high-frequency range, and therefore can possess excellent dielectric properties.

[0019] Furthermore, the dielectric breakdown voltage (BDV) of the aforementioned polyimide coating, measured according to ASTM D149 standard specifications, can be 230 kV / mm or higher. The lower limit of the aforementioned dielectric breakdown voltage can be 233 kV / mm or higher, 235 kV / mm or higher, 238 kV / mm or higher, 240 kV / mm or higher, 243 kV / mm or higher, 244 kV / mm or higher, 245 kV / mm or higher, 246 kV / mm or higher, 247 kV / mm or higher, 248 kV / mm or higher, or 249 kV / mm or higher, while the upper limit can be, for example, below 300 kV / mm, below 290 kV / mm, below 280 kV / mm, below 270 kV / mm, below 265 kV / mm, or below 260 kV / mm. The polyimide covering of this application can provide a polyimide that can simultaneously meet the requirements of low dielectric constant, heat resistance, insulation, adhesion and mechanical properties at high temperature, thereby preventing partial discharge, local degradation and insulation breakdown when used to cover wires, and providing a highly reliable covering.

[0020] The dielectric breakdown voltage (BDV) described above can be determined using methods known in the industry. In one example, the dielectric breakdown voltage can be determined according to the ASTM D149 standard. A sample can be manufactured from a wire coated with the aforementioned polyamic acid composition, and a PHENIX TECHNOLOGIES 6CCE50-5 can be used as the measuring instrument. After pretreating the manufactured sample in an oven at 100°C to remove moisture, the sample is fixed in the measuring instrument set to room temperature atmosphere. A voltage of 10 kVAc is applied from the lower and upper electrodes, and the alternating voltage is increased from 0 at a certain rate, thereby determining the BDV.

[0021] Furthermore, the polyimide coating according to this application is manufactured by coating a conductor wire with a length of 250 mm with the aforementioned polyimide to create a wire sample coated with the coating. Then, with only the coating (excluding the conductor wire) cut from the center of the sample, the two ends of the sample are stretched by 15%, and the gap length formed by the cut portion of the coating can be less than 5 mm. The gap length can be less than 4.8 mm, less than 4.5 mm, less than 4.3 mm, less than 4.0 mm, less than 3.8 mm, less than 3.5 mm, less than 3.3 mm, less than 3.0 mm, less than 2.8 mm, less than 2.5 mm, less than 2.3 mm, or less than 2.0 mm, with no particular limitation on the lower limit, but it can be 0.01 mm or more, or 0.1 mm or more. The conductor wire can be copper wire. Through the above tensile test, the polyimide coating of this application can effectively ensure the adhesion and flexibility of the polyimide coating to the conductor wire.

[0022] This application provides a polyimide that simultaneously satisfies the aforementioned dielectric breakdown voltage, dielectric constant, and physical performance values ​​in the tensile test, thereby providing a polyimide that can simultaneously satisfy low dielectric properties, heat resistance, insulation, adhesion, and high-temperature mechanical properties. Thus, when used to cover electrical wires, it can provide a highly reliable cover by preventing partial discharge, localized degradation, and insulation breakdown.

[0023] Furthermore, the aforementioned diamine monomer may include compounds represented by the following chemical formula 1. In this application, by using a diamine monomer containing a specific structure, insulation breakdown and partial discharge can be prevented, while achieving adhesion and flexibility to the covered object.

[0024] [Chemical Formula 1]

[0025]

[0026] In the above chemical formula 1, A1 and A2 can each independently be an ether group, an ester group, or an amide group. A1 and A2 can be attached to the aromatic ring by removing one hydrogen atom from the aromatic ring. Considering the three-dimensional structure, A1 and A2 can be attached to the meta or para position based on an amino group. X can represent a single bond, an alkylene group, an alkylidene group, an aryl group, or the following chemical formula 2.

[0027] [Chemical Formula 2]

[0028]

[0029] In Formula 2 above, Q can be oxygen, carbonyl, alkyl carbonyl, single bond, alkylene, alkylidene, or sulfonyl. In Formula 2 above, the * linked to the aromatic ring indicates a linker group in which one hydrogen atom in the aromatic ring is removed, thus linking the structure of Formula 2 to A1 or A2 of Formula 1. Considering the three-dimensional structure, the linker group can be linked to the meta or para position based on Q. Q can have alkyl, alkenyl, or alkynyl substituents. Alternatively, Q can have fluorine-substituted alkyl, alkenyl, or alkynyl substituents. In one example, when Q is alkylene, it can have one or two alkyl groups, or more than two and less than five alkyl groups.

[0030] In this specification, the term "single bond" can refer to a bond that connects two atoms without any atoms present. For example, in the above chemical formula 1, when X is a single bond, A1 and A2 can be directly connected to each other.

[0031] In this specification, unless otherwise specified, the term "alkyl" may refer to an alkyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The aforementioned alkyl groups may have a straight-chain, branched, or cyclic structure and may optionally be substituted with one or more substituents. For example, the aforementioned substituents may be polar functional groups, etc.

[0032] In this specification, unless otherwise specified, the term "alkenyl" may refer to an alkenyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The aforementioned alkenyl groups may have a straight-chain, branched, or cyclic structure, and may optionally be substituted by one or more substituents. For example, the aforementioned substituents may be polar functional groups, etc.

[0033] In this specification, unless otherwise specified, the term "alkynyl" may refer to an alkynyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The aforementioned alkynyl group may have a straight-chain, branched, or cyclic structure, and may optionally be substituted by one or more substituents. For example, the aforementioned substituents may be polar functional groups, etc.

[0034] In this specification, unless otherwise specified, the term "alkylene" may refer to an alkylene having 2 to 30 carbon atoms, 2 to 25 carbon atoms, 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, or 2 to 8 carbon atoms. The aforementioned alkyl group may have a straight-chain, branched, or cyclic structure, and may optionally be substituted with one or more substituents. For example, the aforementioned substituents may be polar functional groups, etc.

[0035] In this specification, unless otherwise specified, the term "alkylidene" may refer to an alkylidene group having 2 to 30 carbon atoms, 2 to 25 carbon atoms, 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, or 2 to 8 carbon atoms. The aforementioned alkylidene groups may have a straight-chain, branched, or cyclic structure, and may optionally be substituted by one or more substituents. For example, the aforementioned substituents may be polar functional groups, etc.

[0036] In one example, the compound of Formula 1 described above may be included in the diamine monomer component at a rate of 99 mol% or less. In embodiments, the content of the compound of Formula 1 in the entire diamine monomer component of the composition may be 95 mol% or less, 90 mol% or less, 85 mol% or less, 80 mol% or less, 75 mol% or less, 70 mol% or less, 65 mol% or less, 60 mol% or less, 55 mol% or less, 50 mol% or less, 45 mol% or less, 40 mol% or less, 38 mol% or less, 35 mol% or less, 33 mol% or less, 31 mol% or less, or 25 mol% or less. The content range is 20 mol% or less, or 14 mol% or less. For example, the lower limit can be 5 mol% or more, 8 mol% or more, 9 mol% or more, 10 mol% or more, 12 mol% or more, 15 mol% or more, 18 mol% or more, 20 mol% or more, 23 mol% or more, 25 mol% or more, 28 mol% or more, 33 mol% or more, 38 mol% or more, 43 mol% or more, 48 mol% or more, 53 mol% or more, 58 mol% or more, 63 mol% or more, or 68 mol% or more. In this application, by adjusting the content range of compounds having the structure of the above-described chemical formula 1, the polymerized polyimide resin can achieve excellent heat resistance, electrical properties, flexibility, and adhesion to the adhered substrate.

[0037] In embodiments of this application, the diamine monomer component may further include a compound of chemical formula 3.

[0038] [Chemical Formula 3]

[0039]

[0040] In the above chemical formula 3, R can represent a single bond, ether group, ester group, amide group, carbonyl group, alkyl carbonyl group, alkylene group, alkylidene group, or aryl group. The structure of the above chemical formula 3 has a structure other than that of compounds having the structure of the above chemical formula 1.

[0041] The compound of the above chemical formula 3 may be included in the diamine monomer component at a rate of 5 mol% or more. In embodiments, the content of the compound of Formula 3 in the entire diamine monomer component of the composition can be 10 mol% or more, 15 mol% or more, 20 mol% or more, 25 mol% or more, 30 mol% or more, 35 mol% or more, 40 mol% or more, 45 mol% or more, 50 mol% or more, 55 mol% or more, 60 mol% or more, 63 mol% or more, 65 mol% or more, 68 mol% or more, 70 mol% or more, 80 mol% or more, 85 mol% or more, or 88 mol% or more, with an upper limit, for example, less than 95 mol% or less, less than 93 mol% or less, less than 91 mol% or less, less than 85 mol% or less, less than 80 mol% or less, less than 78 mol% or less, less than 75 mol% or less, less than 73 mol% or less, less than 71 mol% or less, less than 68 mol% or less, less than 63 mol% or less, less than 58 mol% or less, less than 53 mol% or less, less than 48 mol% or less, less than 43 mol% or less, less than 38 mol% or less, less than 33 mol% or less, or less than 28 mol%. Furthermore, based on 100 parts by weight of the compound of chemical formula 3, the content of the compound of chemical formula 1 relative to 100 parts by weight of the compound of chemical formula 3 can be from 5 parts by weight to 150 parts by weight. Within the aforementioned range, the lower limit can be 7 parts by weight or more, 9 parts by weight or more, 10 parts by weight or more, 11 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, 25 parts by weight or more, 30 parts by weight or more, 33 parts by weight or more, 35 parts by weight or more, 38 parts by weight or more, 40 parts by weight or more, 42 parts by weight or more, 45 parts by weight or more, 50 parts by weight or more, 55 parts by weight or more, 60 parts by weight or more, 65 parts by weight or more, 70 parts by weight or more, 75 parts by weight or more, 80 parts by weight or more, 85 parts by weight or more, 90 parts by weight or more, 95 parts by weight or more, 100 parts by weight or more, or 1 0.05 parts by weight or more, with upper limits such as 145 parts by weight or less, 140 parts by weight or less, 135 parts by weight or less, 130 parts by weight or less, 125 parts by weight or less, 120 parts by weight or less, 115 parts by weight or less, 110 parts by weight or less, 108 parts by weight or less, 103 parts by weight or less, 98 parts by weight or less, 93 parts by weight or less, 88 parts by weight or less, 83 parts by weight or less, 78 parts by weight or less, 73 parts by weight or less, 68 parts by weight or less, 63 parts by weight or less, 58 parts by weight or less, 53 parts by weight or less, 50 parts by weight or less, 48 ​​parts by weight or less, 45 parts by weight or less, 43 parts by weight or less, 40 parts by weight or less, 37 parts by weight or less, 34 parts by weight or less, 31 parts by weight or less, 28 parts by weight or less, 23 parts by weight or less, 18 parts by weight or less, or 13 parts by weight or less.In the polyimide resin according to this application, two or more diamines are used, and by adjusting the content ratio of each diamine, corona resistance can be imparted, and the adhesion between the conductor and the cover and the flexibility of the cover can be improved.

[0042] For example, the diamine monomers according to this application are aromatic diamines, which can be classified as follows and illustrated with examples.

[0043] 1) As a diamine having a benzene core in its structure, such as 1,4-diaminobenzene (or p-phenylenediamine, PDA), 1,3-diaminobenzene, 2,4-diaminotoluene, 2,6-diaminotoluene or 3,5-diaminobenzoic acid, i.e., a diamine having a relatively rigid structure;

[0044] 2) Examples include 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, and bis(4-aminophenyl) Sulfides, 4,4'-diaminobenzoylaniline, 3,3'-dichlorobenzidine, 3,3'-dimethylbenzidine (or o-benzidine), 2,2'-dimethylbenzidine (or m-toluidine), 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether (or diphenylamine oxide, ODA), 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-Diaminodiphenyl sulfide, 3,3'-Diaminodiphenyl sulfone, 3,4'-Diaminodiphenyl sulfone, 4,4'-Diaminodiphenyl sulfone, 3,3'-Diaminobenzophenone, 4,4'-Diaminobenzophenone, 3,3'-Diamino-4,4'-Dichlorobenzophenone, 3,3'-Diamino-4,4'-Dimethoxybenzophenone, 3,3'-Diaminodiphenylmethane, 3,4'-Diaminodiphenylmethane, 4,4'-Diaminodiphenylmethane, 2,2-Bis(3- Diamines having two benzene rings in their structure, such as aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide or 4,4'-(1,3-propadiyl)dioxydiphenylamine (PDDA);

[0045] 3) Examples include 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (or TPE-R), 1,4-bis(3-aminophenoxy)benzene (or TPE-Q), 1,4-bis(4-aminophenoxy)benzene (or TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-bis(4-phenylphenoxy)benzophenone. Diamines having three benzene rings in their structure, such as ketones, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3-bis(3-aminophenyl sulfone)benzene, 1,4-bis(4-aminophenyl sulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, or [3-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (p-BABB).

[0046] Examples include 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl]one, and bis[3-(4-aminophenoxy)phenyl]ketone. [4-(3-aminophenoxy)phenyl] ketone, bis[4-(4-aminophenoxy)phenyl] ketone, bis[3-(3-aminophenoxy)phenyl] sulfide, bis[3-(4-aminophenoxy)phenyl] sulfide, bis[4-(3-aminophenoxy)phenyl] sulfide, bis[4-(4-aminophenoxy)phenyl] sulfide, bis[3-(3-aminophenoxy)phenyl] sulfone, bis[3-(4-aminophenoxy)phenyl] sulfone, bis[4-(3-aminophenoxy)phenyl] sulfone, bis[4- [4-aminophenoxy]phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]phenyl Diamines having four benzene rings in their structure, such as 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, or 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.

[0047] Preferably, the compound of Formula 1 can be 4,4'-(1,3-propanediyl)dioxydiphenylamine (PDDA) or [3-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (p-BABB), and the compound of Formula 3 can be 4,4'-diaminodiphenyl ether (or diphenylamine oxide, ODA).

[0048] On the other hand, the dianhydride monomer contained in the polyimide resin according to this application can be an aromatic tetracarboxylic dianhydride. The aforementioned dianhydride monomer component can have one aromatic ring or two or more aromatic rings. For example, the upper limit for the number of aromatic rings can be five.

[0049] Examples of the aforementioned aromatic tetracarboxylic dianhydrides may include pyromellitic dianhydride (or PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (or BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (or a-BPDA), oxydiphenyl dianhydride (or ODPA), diphenyl sulfone-3,4,3',4'-tetracarboxylic dianhydride (or DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride (or BTDA), bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2 1,3-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(triphenyltriacrylic acid monoester anhydride), p-biphenylenebis(triphenyltriacrylic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phenyl dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phenyl dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride, or 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride, etc.

[0050] Preferably, the above-mentioned aromatic tetracarboxylic dianhydride can be pyromellitic dianhydride (or PMDA).

[0051] In embodiments of this application, the polyimide coating may further comprise a silane compound. For example, the silane compound may be one or more compounds selected from the group consisting of epoxy compounds, amine compounds, and thiols. Specifically, the epoxy compound may include glycidoxypropyl trimethoxysilane (GPTMS), the amine compound may include (3-Aminopropyl)trimethoxy-silane (APTMS), and the thiols may include mercapto-propyl-trimethoxysilane (MPTMS), but are not limited thereto. Additionally, the silane compound may include alkoxysilane compounds such as dimethyldimethoxysilane (DMDMS), methyltrimethoxysilane (MTMS), methyltriethoxysilane (MTES), or tetraethoxysilane (TEOS).

[0052] Preferably, the silane compound can be an ammonia-based silane compound.

[0053] Based on 100 parts by weight of polyimide, the content of the silane compound can be from 0.01 parts by weight to 1 part by weight. In embodiments, the content ratio of the silane compound relative to 100 parts by weight of polyamic acid can be 0.03 parts by weight or more, 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, 0.15 parts by weight or more, or 0.18 parts by weight or more, with upper limits, for example, less than 0.8 parts by weight, less than 0.5 parts by weight, less than 0.3 parts by weight, less than 0.23 parts by weight, or less than 0.15 parts by weight. In this application, by including the above-mentioned silane compound, the electrical properties are maintained together with the polyimide resin having the above-mentioned specific structure, while the adhesion to the adhered object is improved.

[0054] In one embodiment, the molecular weight of the polyimide resin can be from 10,000 g / mol to 50,000 g / mol or from 15,000 g / mol to 30,000 g / mol. The weight-average molecular weight refers to the converted value of standard polystyrene or polymethyl methacrylate (PMMA) as determined by gel permeation chromatography (GPC).

[0055] In one example, in this application, elongation can be evaluated to indirectly determine the properties of the coating. The elongation of the polyimide described above can be 70% or more, and in embodiments, it can be 72% or more, 73% or more, 75% or more, 78% or more, 80% or more, 83% or more, 85% or more, 87% or more, 90% or more, 93% or more, 100% or more, 110% or more, 120% or more, 130% or more, or 140% or more, with upper limits, for example, less than 150%, less than 148%, less than 145%, less than 140%, less than 130%, less than 120%, less than 110%, less than 100%, less than 98%, less than 95%, less than 90%, less than 85%, or less than 80%. The coating applied to the wire as described above can also exhibit mechanical properties similar to these mechanical properties.

[0056] In one example, the adhesion strength of the polyimide coating to copper can be 0.65 N / cm or higher. This adhesion strength can be measured after the polyamic acid composition is manufactured into a film (10 mm width × 50 mm height × 20 μm thickness). The adhesion strength can be measured at a temperature of 23°C, a peel angle of 180°, and a peel speed of 20 mm / min.

[0057] In embodiments of this application, the partial discharge initiation voltage (PDIV) of the polyimide coating, as measured according to ASTM 2275-01 standard specifications, can be 800 Vp or higher. In embodiments, the lower limit of the PDIV can be 800 Vp or higher, 820 Vp or higher, 830 Vp or higher, or 850 Vp or higher, and the upper limit can be 1000 Vp or lower than 950 Vp.

[0058] Furthermore, the aforementioned partial discharge initiation voltage (PDIV) can be determined using methods known in the industry. For example, according to ASTM 2275-01, samples twisted into two rows are manufactured by applying a load and twisting to the ends of a pair of samples of a manufactured insulated wire. Then, a voltage at a frequency of 50 Hz to 60 Hz is applied to the bare conductors at both ends of the samples at a constant speed, and the voltage at which partial discharge (above 100 pC) occurs is recorded.

[0059] Furthermore, this application relates to a polyimide precursor composition. The aforementioned polyimide precursor composition may be a precursor composition for the aforementioned polyimide coating, or it may be a polyamic acid composition.

[0060] The solid content of the polyamic acid composition according to this application can be from 10% to 50% by weight. The aforementioned solid content can be 13% or more by weight, 15% or more by weight, 18% or more by weight, 20% or more by weight, 25% or more by weight, or 28% or more by weight, with upper limits, for example, less than 48% by weight, less than 45% by weight, less than 43% by weight, less than 40% by weight, less than 38% by weight, less than 35% by weight, less than 33% by weight, or less than 30% by weight. This application can achieve the desired physical properties and viscosity within the above ranges.

[0061] In this application, the above-mentioned polyamic acid composition may include a first solvent as an organic solvent.

[0062] There are no particular restrictions on the organic solvents used, as long as they can dissolve polyamic acid. For example, the organic solvents mentioned above can be aprotic polar solvents.

[0063] For example, examples of the aforementioned aprotic polar solvents may include amide solvents such as N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc) or dimethylpropionamide (DMPA), phenolic solvents such as p-chlorophenol and o-chlorophenol, N-methylpyrrolidone (NMP), γ-butyrolactone (GBL) and diethylene glycol dimethyl ether (Diglyme), which may be used alone or in combination of two or more.

[0064] In one example, the polyamic acid composition of this application may further include a second solvent having at least one polar functional group selected from the group consisting of hydroxyl, carboxyl, alkoxy, ester, and ether groups. The second solvent may also be an organic solvent, but the first solvent and the second solvent may be different components.

[0065] In one embodiment, in addition to the monomers contained in the polymerization unit, the dianhydride monomer may also contain unpolymerized monomers with an open-ring structure. That is, a portion of the dianhydride monomer may be included in the polymerization unit, or a portion of the dianhydride monomer may not be included in the polymerization unit. The dianhydride monomer not included in the polymerization unit may have a ring-opening structure obtained by using the organic solvent according to this application. The polyamic acid composition according to this application can exist in the form of an aromatic carboxylic acid having two or more carboxylic acids in the unpolymerized state of the dianhydride monomer. The aromatic carboxylic acid exists as a monomer before curing, thereby reducing the viscosity of the entire polyamic acid composition and improving processability. After curing, the aromatic carboxylic acid having two or more carboxylic acids polymerizes as a dianhydride monomer in the main chain, thereby increasing the total polymer chain length. When the polymer is applied to a coating, it can achieve excellent heat resistance, dimensional stability, and mechanical properties.

[0066] Specifically, during the heat treatment process of imidizing the above-mentioned polyamic acid composition into polyimide, the aromatic carboxylic acid having two or more carboxylic acids is converted into dianhydride monomers through a ring-closing dehydration reaction, thereby reacting with the terminal amine groups of the polyamic acid chain or the polyimide chain, resulting in an increase in polymer chain length. As a result, the dimensional stability and thermal stability at high temperatures of the manufactured polyimide film can be improved, and the mechanical properties at room temperature can be improved.

[0067] In one example, as described above, the polyamic acid composition of this application may contain a second solvent, the content of which in the entire polyamic acid composition may be from 0.01 wt% to 10 wt%. For example, the lower limit of the second solvent may be 0.015 wt%, 0.03 wt%, 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.3 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, or 2 wt% or more, and the upper limit may be, for example, 10 wt%, 9 wt%, 8 wt%, 7 wt%, 6 wt%, 5.5 wt%, 5.3 wt%, 5 wt%, 4.8 wt%, 4.5 wt%, 4 wt%, 3 wt%, 2.5 wt%, 1.5 wt%, 1.2 wt%, 0.95 wt%, or 0.4 wt% or less. Furthermore, the content of the first solvent in the entire polyamic acid composition may be from 60 wt% to 95 wt%. For example, the lower limit of the first solvent can be 65 wt%, 68 wt%, 70 wt%, 73 wt%, 75 wt%, 78 wt%, or 80 wt% or more, and the upper limit can be 93 wt%, 90 wt%, 88 wt%, 85 wt%, 83 wt%, 81 wt%, or 79 wt% or less. The polyamic acid composition according to this application includes a dianhydride monomer component and a diamine monomer component, the two monomers forming polymeric units with each other. However, a portion of the dianhydride monomer is ring-opened by the organic solvent and cannot participate in the polymerization reaction. The unpolymerized, ring-opened dianhydride monomer acts as a diluent monomer, thereby adjusting the viscosity of the entire polyamic acid composition to a lower level. The dianhydride monomer having the above-mentioned ring-opening structure participates in the imidization reaction, thereby achieving a polyimide with heat resistance, flexibility, low dielectric constant, and adhesion as a desired coating.

[0068] In one example, the second solvent described above can dissolve the dianhydride monomer in an amount of less than 1.5 g / 100 g. That is, the solubility of the second solvent relative to the dianhydride monomer can be less than 1.5 g / 100 g. The upper limit of the above solubility range can be, for example, below 1.3g / 100g, 1.2g / 100g, 1.1g / 100g, 1.0g / 100g, 0.9g / 100g, 0.8g / 100g, 0.7g / 100g, 0.6g / 100g, 0.5g / 100g, 0.4g / 100g, 0.3g / 100g, 0.25g / 100g, 0.23g / 100g, 0.21g / 100g, 0.2g / 100g, or 0.15g / 100g, and the lower limit can be, for example, above 0g / 100g, 0.01g / 100g, 0.05g / 100g, 0.08g / 100g, 0.09g / 100g, or 0.15g / 100g. This application provides a polyamic acid composition with desired physical properties by including a second solvent having low solubility for the dianhydride monomer or unpolymerized dianhydride monomer contained as a polymerization unit. If the physical properties measured in this application are temperature-dependent, they may be measured at room temperature (23°C) unless otherwise specified.

[0069] In embodiments of this application, for example, the solubility of the first solvent relative to the dianhydride monomer can be 1.5 g / 100 g or more. The lower limit of the solubility can be, for example, 1.6 g / 100 g, 1.65 g / 100 g, 1.7 g / 100 g, 2 g / 100 g, 2.5 g / 100 g, 5 g / 100 g, 10 g / 100 g, 30 g / 100 g, 45 g / 100 g, 50 g / 100 g, or 51 g / 100 g or more, and the upper limit can be, for example, 80 g / 100 g, 70 g / 100 g, 60 g / 100 g, 55 g / 100 g, 53 g / 100 g, 48 g / 100 g, 25 g / 100 g, 10 g / 100 g, 5 g / 100 g, or 3 g / 100 g or less. The solubility of the first solvent can be higher than that of the second solvent.

[0070] In one example, the boiling point of the first solvent may be above 150°C, and the boiling point of the second solvent may be below the boiling point of the first solvent. That is, the boiling point of the first solvent may be higher than the boiling point of the second solvent. The boiling point of the second solvent may be equal to or greater than 30°C and less than 150°C. The lower limit of the boiling point of the first solvent may be, for example, above 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, or 201°C, and the upper limit may be, for example, below 500°C, 450°C, 300°C, 280°C, 270°C, 250°C, 240°C, 230°C, 220°C, 210°C, or 205°C. Furthermore, the lower limit of the boiling point of the aforementioned second solvent can be, for example, 35°C, 40°C, 45°C, 50°C, 53°C, 58°C, 60°C, or 63°C or higher, and the upper limit can be, for example, 148°C, 145°C, 130°C, 120°C, 110°C, 105°C, 95°C, 93°C, 88°C, 85°C, 80°C, 75°C, 73°C, 70°C, or 68°C or lower. In this application, polyimides with desired physical properties can be prepared by using two solvents with different boiling points.

[0071] As the first solvent according to this application, there are no particular limitations as long as it is a solvent capable of dissolving polyamic acid. The first solvent can also be a polar solvent. For example, the first solvent can be an amide solvent such as N,N-dimethylformamide, N,N-dimethylacetamide, or N-methylpyrrolidone; for example, the first solvent may have an amide group or a ketone group in its molecular structure. The polarity of the first solvent can be lower than that of the second solvent.

[0072] As an example, the first solvent mentioned above can be an aprotic polar solvent. The second solvent can be either an aprotic polar solvent or a protic polar solvent. For example, the second solvent may include alcohol solvents such as methanol, ethanol, 1-propanol, butanol, isobutanol, or 2-propanol; ester solvents such as methyl acetate, ethyl acetate, or isopropyl acetate; carboxylic acid solvents such as formic acid, acetic acid, propionic acid, butyric acid, or lactic acid; ether solvents such as dimethyl ether, diethyl ether, diisopropyl ether, or dimethoxyethane methyl tert-butyl ether; dimethyl carbonate; methyl methacrylate; or propylene glycol monomethyl ether acetic acid.

[0073] As previously stated, this application may simultaneously contain both the first solvent and the second solvent. In this case, the content of the first solvent may be greater than the content of the second solvent. Furthermore, based on 100 parts by weight of the first solvent, the second solvent may be contained in a ratio of 0.01 parts by weight to 10 parts by weight. For example, the lower limit of the aforementioned content ratio may be 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.1 parts by weight, 0.3 parts by weight, 0.5 parts by weight, 0.8 parts by weight, 1 part by weight, or 2 parts by weight or more, and the upper limit may be, for example, 8 parts by weight, 6 parts by weight, 5 parts by weight, 4.5 parts by weight, 4 parts by weight, 3 parts by weight, 2.5 parts by weight, 1.5 parts by weight, 1.2 parts by weight, 0.95 parts by weight, 0.4 parts by weight, 0.15 parts by weight, or 0.09 parts by weight or less.

[0074] The polyamic acid composition of this application can be a composition with low viscosity characteristics. The polyamic acid composition of this application exhibits low viscosity at 23°C and 1 second... -1 The viscosity, measured under certain shear rate conditions, can be below 10,000 cP or 9,000 cP. The lower limit is not particularly limited, but can be above 500 cP or 1,000 cP. For example, the above viscosity can be measured using a Haake Rheostress 600, and can be measured under conditions of a shear rate of 1 / s, a temperature of 23°C, and a plate gap of 1 mm. In this application, by adjusting the above viscosity range, a precursor composition with excellent processability is provided, thereby enabling the formation of a coating with desired physical properties when coating conductive wires.

[0075] This application also relates to a method for preparing a polyamic acid composition. The above-described preparation method can be a method for preparing the aforementioned polyamic acid composition.

[0076] The preparation method of the above-mentioned polyamic acid composition may include the step of separately adding at least one of the dianhydride monomer and the diamine monomer, and adding them at least twice.

[0077] The above-mentioned polyamic acid composition can be prepared by polymerizing dianhydride monomers and diamine monomers in an organic solvent.

[0078] In addition, the dianhydride monomer and the diamine monomer mentioned above can be added in powder, lump, or solution form. Preferably, they are added in powder form at the beginning of the reaction to carry out the reaction, and then added in solution form to adjust the polymerization viscosity.

[0079] For example, dianhydride monomers and diamine monomers can be added in powder form to react, and then dianhydride can be added in solution form to react until the viscosity of the polyamic acid composition reaches a certain range.

[0080] On the other hand, as a method for preparing the above-mentioned polyamic acid composition, the present invention provides a method for preparing a polyamic acid composition, wherein at least one of a dianhydride monomer and a diamine monomer is added to the above-mentioned organic solvent and dissolved, and at least one of a dianhydride monomer and a diamine monomer is added separately to the above-mentioned organic solvent, at least on both sides, thereby polymerizing the polyamic acid and stirring.

[0081] The equivalence ratio of the diamine monomer to the dianhydride monomer can be adjusted by separating the addition of the dianhydride monomer and the diamine monomer.

[0082] Specifically, at least one of the dianhydride monomers and diamine monomers can be added separately, in which case the addition is done at least twice and no more than five times.

[0083] For example, the polyimide coating according to this application can be coated and cured onto the surface of a conductor. In one example, the preparation method of the coating may include the following steps: coating a polyamic acid composition onto the surface of the conductor; and imidizing the polyamic acid composition coated on the surface of the conductor. The conductor may be a copper wire made of copper or a copper alloy, but may also include conductors made of other metallic materials such as silver wire or various gold-plated metal wires such as aluminum wire or tin-plated wire. The thickness of the conductor and the coating may conform to KSC 3107 standard. The diameter of the conductor may be in the range of 0.3 mm to 3.2 mm, and the standard film thickness of the coating (average of the maximum and minimum film thickness) is 21 μm to 194 μm for type 0, 14 μm to 169 μm for type 1, and 10 μm to 31 μm for type 2. The cross-sectional shape of the conductor may be a round wire, a flat wire, a hexagonal wire, etc., but is not limited thereto.

[0084] This application may also provide a covered wire, the covered wire comprising a polyimide cover prepared by coating the aforementioned polyamic acid composition onto the surface of a wire and imidizing it. In one embodiment, the covered wire may include: a wire; and a cover formed by coating the aforementioned polyimide onto the surface of the wire and imidizing it.

[0085] Additionally, this application can provide an electronic device that includes the aforementioned covering wires. For example, an example of such an electronic device could be an electric motor.

[0086] The effects of the invention

[0087] As described above, this application can provide a polyimide cover that has low dielectric constant properties, can prevent insulation breakdown and partial discharge, and also improves the adhesion between the conductor and the cover and the flexibility of the cover. Detailed Implementation

[0088] The best way to implement the invention

[0089] The present invention will now be described in more detail through embodiments of the present invention and comparative examples of non-the present invention, but the scope of the present invention is not limited to the following embodiments.

[0090] <Example 1>

[0091] Dimethylacetamide was added as a solvent to a 1L reactor under a nitrogen atmosphere.

[0092] After setting the temperature to 23°C to 50°C, 95 parts by weight of pyromellitic dianhydride (PMDA) as a dianhydride monomer, 90 parts by weight of 4,4'-diaminodiphenyl ether (4,4'-ODA) as a diamine monomer, and 10 parts by weight of 4,4'-(1,3-propanediyl)dioxydiphenylamine (PDDA) were added and dissolved. Five parts by weight of the above-mentioned pyromellitic dianhydride (PMDA) were added in three portions at 30-minute intervals to polymerize polyamic acid.

[0093] The polyamic acid composition was prepared by mixing 0.2 parts by weight of an amino silane compound PAPTES (Dow's Z-6883 silane) as a silane compound into the prepared polyamic acid composition.

[0094] Preparation of polyimide coatings

[0095] In a coating curing oven, using the prepared polyamic acid composition, the coating thickness is adjusted to between 5 μm and 15 μm on a copper wire with a conductor diameter of 1 mm. The minimum and maximum temperatures of the coating curing oven are adjusted to between 350°C and 550°C, and the covering speed of the copper wire is adjusted to between 12 m / min and 32 m / min. Under these conditions, a wire (covered wire) with a polyimide coating thickness of 33 μm to 35 μm is prepared.

[0096] <Example 2>

[0097] Except for the addition of 70 parts by weight of 4,4'-ODA and 30 parts by weight of 4,4'-(1,3-propanediyl)dioxydiphenylamine (PDDA) as diamine monomers, the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Example 1.

[0098] <Example 3>

[0099] Except that the silane compounds were not mixed, the polyamic acid composition, polyimide coating, and covered wires were prepared in the same manner as in Example 2.

[0100] <Example 4>

[0101] The polyamic acid composition, polyimide coating, and covered wire were prepared in the same manner as in Example 3, except that 30 parts by weight of [3-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate (p-BABB) was mixed in place of 4,4'-(1,3-propanediyl)dioxydiphenylamine (PDDA) as the diamine monomer.

[0102] <Comparative Example 1>

[0103] Except that 100 parts by weight of 4,4'-ODA was added as a diamine monomer and dissolved, and 100 parts by weight of PMDA was added as a dianhydride monomer, the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Example 1.

[0104] <Comparative Example 2>

[0105] Except that the silane compound was not mixed, the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Comparative Example 1.

[0106] <Comparative Example 3>

[0107] Except for mixing 30 parts by weight of 4,4'-diaminobenzoylaniline (DABA) as a diamine monomer to replace 4,4'-(1,3-propanediyl)dioxydiphenylamine (PDDA), the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Example 2.

[0108] <Comparative Example 4>

[0109] Except for the addition of 70 parts by weight of PMDA and 30 parts by weight of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride (BPDA) as dianhydride monomers in place of 100 parts by weight of PMDA, the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Comparative Example 2.

[0110] <Comparative Example 5>

[0111] Except for the addition of 70 parts by weight of PMDA and 30 parts by weight of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) as dianhydride monomers in place of 100 parts by weight of PMDA, the polyamic acid composition, polyimide coating and covered wire were prepared in the same manner as in Comparative Example 2.

[0112] <Experimental Example 1: Adhesive Force>

[0113] Copper foil (Cu foil) was cut to a certain size and fixed to a glass substrate with adhesive tape. The polyamic acid composition prepared in the examples and comparative examples was coated onto the copper foil, and a film with a certain thickness (width 10 mm × height 50 mm × thickness 20 μm) was formed by spin coating. The coated polyamic acid composition was cured, and the cured polyimide was coated onto the copper foil.

[0114] UTM (Peel strength) was determined by peeling the copper foil layer and the polyimide cured layer. The polyimide cured layer was fixed to the upper fixture, and the copper foil layer to the lower fixture. At room temperature of 23°C, force was applied at a peel angle of 180° and a peel speed of 20 mm / min to determine the adhesive strength.

[0115] <Experiment Example 2: Tensile Test>

[0116] To confirm the adhesion between the conductor and the covering, tensile tests were performed on the polyimide coverings of the wires manufactured in the Examples and Comparative Examples, and the results are shown in Table 1 below.

[0117] Specifically, for a straight wire sample with a free measurement length of 200mm to 250mm, the center portion is cut only from the covering material (only the portion of the covering material excluding the copper wire). The two ends of the sample are then stretched by 15%.

[0118] Measure the length of the gap formed by the opening of the cut portion of the covering.

[0119] <Experimental Example 3: Elongation>

[0120] The polyamic acid compositions prepared in the examples and comparative examples were formed into film shapes and cured.

[0121] After the polyimide film was cut into dimensions of 10 mm width and 50 mm length, the elongation was determined using an Instron 5564 UTM instrument from Instron Corporation according to the ASTM D-882 method.

[0122] <Experiment Example 4: Dielectric Constant Determination>

[0123] The dielectric constant of the polyimide coatings prepared in the above examples and comparative examples was determined at 10 GHz using an EVA vector network analyzer (E5063A, Keysight Technologies) at 23°C and 50% RH.

[0124] <Experimental Example 5: Evaluation of Dielectric Breakdown Voltage (BDV)>

[0125] The BDV values ​​of the polyimide coatings prepared in the above examples and comparative examples were determined according to ASTM D149 specifications.

[0126] Measurement equipment: PHENIX TECHNOLOGIES 6CCE50-5

[0127] After pretreating the prepared sample in an oven at 100°C to remove moisture, the sample was fixed in the aforementioned measuring device set to room temperature atmosphere, and a voltage of 10 kVAc was applied from the lower electrode and the upper electrode, increasing at a constant rate from 0, and the BDV was measured.

[0128] <Experimental Example 6: Evaluation of Partial Discharge Initiation Voltage (PDIV)>

[0129] The voltage at which partial discharge begins was measured by applying a voltage having a 60Hz sine wave to the polyimide coating according to the various embodiments and comparative examples at room temperature. Here, the voltage at which a charge of 100pC or more is detected is measured as the applied voltage is increased.

[0130] <Experimental Example 7: Crack Resistance Evaluation>

[0131] According to section 7.1.2 of JIS C 3003, the crack resistance of the polyimide coatings according to the various examples and comparative examples was evaluated. Specifically, if cracks occurred in three samples formed by bending a mandrel with a diameter of 3W, which is equivalent to three times the conductor width W, and in three samples formed by bending a mandrel with a diameter of 3T, which is equivalent to three times the conductor height T, then the sample was considered unqualified (fail).

[0132] Table 1

[0133]

Claims

1. A polyimide coating, characterized in that, This includes polyimides having dianhydride monomer components and diamine monomer components as polymerization units, as well as silane compounds; After curing, the dielectric constant Dk in the 10GHz band is less than 3.

6. The dielectric breakdown voltage (BDV) measured according to ASTM D149 standard specifications is above 230 kV / mm. A wire sample covered with a covering is manufactured by covering the above-mentioned polyimide with a conductor wire having a length of 250 mm. Then, with the covering except for the conductor wire cut in the center of the sample, when the two ends of the sample are stretched by 15%, the gap length formed by the cut portion of the covering is less than 5 mm. The dianhydride monomer is pyromellitic dianhydride. The diamine monomer component is 4,4' Diaminodiphenyl ether and 4,4' (1,3 A mixture of propyldioxydiphenylamine, Among them, based on 100 parts by weight of 4,4' Diaminodiphenyl ether, 4,4' (1,3 The content of propyldioxydiphenylamine is 5 to 50 parts by weight.

2. The polyimide coating according to claim 1, characterized in that, Based on 100 parts by weight of polyimide, the content of the above silane compound is from 0.01 parts by weight to 1 part by weight.

3. The polyimide coating according to claim 1, characterized in that, After the polyimide film was cut into dimensions of 10 mm width and 50 mm length, the elongation was measured to be over 70% using an Instron 5564 UTM instrument from Instron Corporation according to the ASTM D-882 method.

4. The polyimide coating according to claim 1, characterized in that, Copper foil was cut to a certain size and fixed to a glass substrate with tape. The prepared polyamic acid composition was coated onto the copper foil and a film with a width of 10 mm × height of 50 mm × thickness of 20 μm was formed by spin coating. The coated polyamic acid composition was cured and a polyimide cured product was coated onto the copper foil. The polyimide cured product layer was fixed on the upper fixture and the copper foil layer was fixed on the lower fixture. At room temperature of 23°C, a force was applied at a peel angle of 180° and a peel speed of 20 mm / min to measure the adhesion force to the copper. The adhesion force was 0.65 N / cm or higher.

5. The polyimide coating according to claim 1, characterized in that, The partial discharge initiation voltage (PDIV) measured according to ASTM 2275-01 standard specifications is above 800 Vp.

6. A type of electrical wire, characterized in that, Includes the polyimide coating according to claim 1.

7. An electronic device, characterized in that, Includes the wire as described in claim 6.

Citation Information

Patent Citations

  • Polyimide resin varnish, and insulated electrical wire, electrical coil, and motor using same

    CN103003332A

  • Polyimide varnish comprising aromatic carboxylic acid for conductor coating and manufacturing method therefor

    CN112585228A

  • Delivery system with improved bioavailability

    JP2011012072A

  • Polyesterimide precursor and polyesterimide

    JP2011021072A

  • KR1020135310000B1