Non-metallic self-lubricating joint prosthesis component and process for its production

By using silicon nitride and sintering aids to prepare non-metallic self-lubricating joint prosthesis components, the problem of high wear rate of joint prostheses was solved, and joint prostheses with long service life and high stability were achieved, reducing the occurrence of adverse reactions.

CN117653784BActive Publication Date: 2026-11-24BEIJING ZHONGAN TAIHUA TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311712460.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2026-11-24
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

Existing joint prostheses have a high wear rate, leading to early failure and adverse reactions, which affects their service life.

Method used

Using silicon nitride as the main raw material, combined with sintering aids and vacuum plasma spraying technology, non-metallic self-lubricating joint prosthesis components are prepared to improve their density and biocompatibility, reduce wear rate, and increase integration with human tissue.

Benefits of technology

It reduces the wear rate of joint prosthesis components, reduces the release of metal ions and the generation of polyethylene particles, improves the service life and stability of the prosthesis, and reduces rejection reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004605178160000051
    Figure BDA0004605178160000051
  • Figure BDA0004605178160000061
    Figure BDA0004605178160000061
  • Figure BDA0004605178160000062
    Figure BDA0004605178160000062
Patent Text Reader

Abstract

This application relates to the field of joint prosthesis technology, specifically disclosing a non-metallic self-lubricating joint prosthesis component and its preparation process. The preparation process of the non-metallic self-lubricating joint prosthesis component includes the following steps: S1, weighing and mixing silicon nitride and a sintering aid to obtain a mixture; S2, adding the mixture to an ethanol solution for ultrasonic dispersion to obtain a dispersion, and adjusting the pH of the dispersion with acetic acid; S3, heating and stirring the dispersion, centrifuging to obtain a precipitate, then vacuum drying and pulverizing the precipitate to obtain a mixed powder; S4, using the mixed powder to prepare the joint prosthesis component; S5, vacuum hot-pressing and sintering the joint prosthesis component, polishing it, and then vacuum plasma spraying its surface to obtain the non-metallic self-lubricating joint prosthesis component. The non-metallic self-lubricating joint prosthesis component provided by this application can effectively reduce the wear rate of joint prostheses and improve their service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of joint prosthesis technology, and in particular to a non-metallic self-lubricating joint prosthesis component and its manufacturing process. Background Technology

[0002] The hip and knee joints are two important weight-bearing joints in the human body, and also the joints with the largest range of motion among weight-bearing joints. In recent years, the number of people suffering from joint diseases in my country has been increasing year by year, with osteoarthritis in the elderly having the highest incidence. Osteoarthritis of the hip and knee joints (degenerative changes and bone hyperplasia of the knee joint) is a common disease in the elderly. In the early stages, the main symptoms are joint pain and discomfort, which worsens after exposure to cold or exertion, and joint swelling is sometimes present. As the local lesions worsen, the joint pain becomes more pronounced, walking becomes difficult, and the patient's quality of life declines significantly.

[0003] For patients with severe joint disease, the most effective treatment to relieve joint pain, improve joint function, correct joint deformities, and achieve long-term joint stability is artificial joint replacement surgery.

[0004] Current limitations of existing joint prosthesis technology include: post-replacement prosthesis wear is one of the key issues affecting prosthesis lifespan. Wear particles are generated in the joint prosthesis components after wear, which may lead to adverse reactions such as joint infection due to osteolysis and joint loosening, and may also affect the stability of joint support after replacement, resulting in early prosthesis wear failure. Summary of the Invention

[0005] In order to solve at least one of the above-mentioned technical problems and develop a joint prosthesis component with low wear rate and long service life, this application provides a non-metallic self-lubricating joint prosthesis component and its manufacturing process.

[0006] On the one hand, the manufacturing process of a non-metallic self-lubricating joint prosthesis component provided in this application includes the following steps: S1, weighing and mixing silicon nitride and sintering aid to obtain a mixture; S2. The mixture obtained in step S1 is added to an ethanol solution with a mass fraction of 75-85% and ultrasonically dispersed to obtain a dispersion. The pH of the dispersion is adjusted to 5-6 with acetic acid. S3. After heating the dispersion obtained in step S2 to 70-80℃ and stirring for 6-8 hours, centrifuge to obtain precipitate, then vacuum dry the precipitate and pulverize it to obtain mixed powder. S4. Use the mixed powder obtained in step S3 to prepare the joint prosthesis component; S5. The joint prosthesis component obtained in step S4 is subjected to vacuum hot pressing sintering, and the sintered joint component is polished. Then, the surface of the joint prosthesis component is coated by vacuum plasma spraying to form a coating, thereby obtaining the non-metallic self-lubricating joint prosthesis component.

[0007] By adopting the above technical solution, this application uses silicon nitride as the main raw material to prepare joint prosthesis components. Silicon nitride has high strength, high hardness, high temperature stability, as well as good insulation and self-lubricating properties. The use of sintering aids can effectively improve the density of silicon nitride ceramics, thereby improving the mechanical properties of the prepared non-metallic self-lubricating joint prosthesis components. Furthermore, the roughness of the sintered and polished non-metallic self-lubricating joint prosthesis components can reach Ra 0.02, which can effectively reduce the wear rate of joint prosthesis components. At the same time, it can be well matched with joint prosthesis components made of ultra-high molecular weight polyethylene, highly cross-linked ultra-high molecular weight polyethylene, and highly cross-linked ultra-high molecular weight polyethylene mixed with vitamin E, effectively reducing the release of metal ions and the generation of polyethylene particles in the joint prosthesis components, thereby avoiding adverse reactions such as infection and joint loosening caused by osteolysis of the joint prosthesis, which is conducive to improving the service life of the prosthesis.

[0008] Optionally, in step S1, 80-90 parts of silicon nitride and 10-20 parts of sintering aid are weighed by weight.

[0009] Optionally, the sintering aids include yttrium oxide, aluminum oxide and magnesium oxide, wherein the mass ratio of yttrium oxide, aluminum oxide and magnesium oxide is (3-6):(2-5):(2-5).

[0010] By adopting the above technical solution, this application limits the amount of silicon nitride and sintering aid, as well as the compounding ratio of the ternary compounded sintering aid. It utilizes alumina and magnesium oxide to improve the density and hardness of silicon nitride, and uses yttrium oxide to enhance the toughness of silicon nitride. Combined with the excellent properties of silicon nitride such as self-lubrication, light weight, strength, biocompatibility and antibacterial properties, the resulting non-metallic self-lubricating joint prosthesis component has excellent mechanical properties and a long service life. At the same time, the joint prosthesis component is lighter and feels better after being implanted into the human body.

[0011] Optionally, in step S2, the ultrasonic frequency is 55-65kHz and the ultrasonic dispersion time is 20-30min.

[0012] By adopting the above technical solution and using ultrasonic dispersion, the mixture can be uniformly dispersed in the ethanol solution to form a suspension, which is beneficial to the dispersion stability of the particles and prevents the aggregation and sedimentation between particles.

[0013] Optionally, in step S3, the particle size of the mixed powder is 200-300 mesh.

[0014] Optionally, in step S4, the joint prosthesis components obtained by mixing the powder are the acetabular cup, liner, femoral head, and femoral stem in the hip joint prosthesis, and the femoral condyle, tibial pad, and tibial support in the knee joint.

[0015] Optionally, in step S4, the method for preparing the joint prosthesis component by mixing the powder includes the following steps: 1) The mixed powder is cold isostatically pressed under a pressure of 200-250MPa to obtain a blank; 2) The blank material is machined to obtain the joint prosthesis component.

[0016] Optionally, in step S4, the method for preparing the joint prosthesis component by mixing powder is 3D printing.

[0017] Optionally, when using 3D printing to prepare joint prosthesis components, a mesh of trabecular bone structure can be directly printed on the surface of the joint prosthesis in contact with the bone.

[0018] By adopting the above technical solution, a grid of trabecular bone structure can be printed on the surface of the joint prosthesis component, which can increase the contact area between the joint prosthesis component and the surrounding bone tissue, and promote the ingrowth and fusion of bone and joint prosthesis.

[0019] Optionally, in step S5, the temperature of vacuum hot pressing sintering is 1300-1800℃ and the pressure is 25-35MPa.

[0020] Optionally, in step S5, the coating material for vacuum plasma spraying is preferably a titanium, titanium + HA, or pure tantalum coating, and the resulting coating thickness is 0.25–1.5 mm.

[0021] By adopting the above technical solution, this application utilizes vacuum plasma spraying of titanium, titanium + HA, or pure tantalum on the surface of joint prosthesis components. This facilitates better bone growth and fusion after implantation, improving the stability and lifespan of the prosthesis components. Simultaneously, titanium, titanium + HA, and pure tantalum possess excellent biocompatibility, enabling them to readily integrate with human tissues and reducing the risk of rejection and infection after joint prosthesis implantation.

[0022] Secondly, this application provides a non-metallic self-lubricating joint prosthesis component prepared by the aforementioned manufacturing process.

[0023] The invention includes at least one of the following beneficial technical effects: 1. This application uses silicon nitride as the main raw material to prepare joint prosthesis components. Silicon nitride has high strength, high hardness, high temperature stability, as well as good insulation and self-lubricating properties. The use of sintering aids can effectively improve the density of silicon nitride ceramics, thereby improving the mechanical properties of the prepared non-metallic self-lubricating joint prosthesis components. Furthermore, the roughness of the sintered and polished non-metallic self-lubricating joint prosthesis components can reach Ra 0.02, which can effectively reduce the wear rate of joint prosthesis components. At the same time, it can be well matched with joint prosthesis components made of ultra-high molecular weight polyethylene, highly cross-linked ultra-high molecular weight polyethylene, and highly cross-linked ultra-high molecular weight polyethylene mixed with vitamin E, effectively reducing the release of metal ions and the generation of polyethylene particles in the joint prosthesis components, thereby avoiding adverse reactions such as infection and joint loosening caused by osteolysis of the joint prosthesis, which is conducive to improving the service life of the prosthesis.

[0024] 2. This application specifies the dosage of silicon nitride and sintering aids, as well as the compounding ratio of the ternary composite sintering aids. It utilizes alumina and magnesium oxide to improve the density and hardness of silicon nitride, and yttrium oxide to enhance its toughness. Combined with the excellent properties of silicon nitride, such as self-lubrication, lightweight, strength, biocompatibility, and antibacterial properties, the resulting non-metallic self-lubricating joint prosthesis component exhibits excellent mechanical properties and a long service life. The joint prosthesis component provided in this application has a density of 3.2 g / cm³. 3 Currently, the joint prosthesis components commonly used in the market are typically made of zirconia or zirconia-toughened high-purity alumina-based composite materials, with a density of 4.4 g / cm³. 3 The joint prosthesis component provided in this application is lighter and provides better proprioception after implantation.

[0025] 3. This application utilizes vacuum plasma spraying of titanium, titanium + HA, or pure tantalum on the surface of joint prosthesis components. This promotes better bone growth and fusion after implantation, improving the stability and lifespan of the prosthesis. Simultaneously, titanium, titanium + HA, and pure tantalum possess excellent biocompatibility, allowing for good compatibility with human tissues and reducing the risk of rejection and infection after joint prosthesis component implantation. Detailed Implementation

[0026] The present application will be further described in detail below with reference to the embodiments.

[0027] This application provides a manufacturing process for a non-metallic self-lubricating joint prosthesis component, comprising the following steps: S1. Weigh and mix silicon nitride and sintering aid to obtain a mixture; S2. The mixture obtained in step S1 is added to an ethanol solution with a mass fraction of 75-85% and ultrasonically dispersed to obtain a dispersion. The pH of the dispersion is adjusted to 5-6 with acetic acid. S3. After heating the dispersion obtained in step S2 to 70-80℃ and stirring for 6-8 hours, centrifuge to obtain precipitate, then vacuum dry the precipitate and pulverize it to obtain mixed powder. S4. Use the mixed powder obtained in step S3 to prepare the joint prosthesis component; S5. The joint prosthesis component obtained in step S4 is subjected to vacuum hot pressing sintering, and the sintered joint component is polished. Then, the surface of the joint prosthesis component is coated by vacuum plasma spraying to form a coating, thereby obtaining the non-metallic self-lubricating joint prosthesis component.

[0028] This application provides a non-metallic self-lubricating joint prosthesis component, which is manufactured using the aforementioned manufacturing process for non-metallic self-lubricating joint prostheses. Specific Implementation

[0029] Silicon nitride: CAS No.: 12033-89-5; Yttrium oxide: CAS No.: 1314-36-9; Alumina: CAS No.: 1344-28-1; Magnesium oxide: CAS No.: 1309-48-4.

[0030] The following are Examples 1-21 and Comparative Examples 1-3 of this application. Examples 1-21 and Comparative Examples 1-3 respectively provide a non-metallic self-lubricating joint prosthesis component and its manufacturing process.

[0031] The non-metallic self-lubricating joint prosthesis components prepared in Examples 1-21 and Comparative Examples 1-3 of this application were subjected to experimental testing. The test items and test methods are as follows: Hardness: Measured using a Vickers hardness tester.

[0032] Bending strength: determined according to test standard ISO 14704:2016.

[0033] Fracture toughness: determined according to test standard ISO 7206-4.

[0034] Volumetric wear rate: determined according to test standard ISO 14242:2014.

[0035] Example 1 A fabrication process for a non-metallic self-lubricating joint prosthesis component includes the following steps: S1. Weigh 850g of silicon nitride and 150g of sintering aid and mix them to obtain a mixture; the sintering aid is yttrium oxide, aluminum oxide and magnesium oxide in a mass ratio of 5:3:4. S2. Add the mixture obtained in step S1 to an 80% ethanol solution and ultrasonically disperse it for 25 minutes at an ultrasonic frequency of 60 kHz to obtain a dispersion. Adjust the pH of the dispersion to 5.5 with acetic acid. S3. After heating the dispersion obtained in step S2 to 75°C and stirring for 7 hours, centrifuge to obtain precipitate. Then, vacuum dry the precipitate, pulverize it, and pass it through a 250-mesh sieve to obtain mixed powder. S4. Using the mixed powder obtained in step S3, a joint prosthesis component is fabricated by 3D printing. S5. The joint prosthesis component obtained in step S4 is subjected to vacuum hot pressing sintering at a temperature of 1500℃ and a pressure of 30MPa. The sintered joint component is then polished, and the surface of the joint prosthesis component is then subjected to vacuum plasma spraying with titanium as the spraying material. The resulting coating thickness is 1mm, thus obtaining the non-metallic self-lubricating joint prosthesis component.

[0036] Examples 2-8 The difference between Examples 2-4 and Example 1 is that the mass ratio of yttrium oxide, aluminum oxide and magnesium oxide in the sintering aid is different from that in Example 1. The differences are shown in Table 1.

[0037] The difference between Examples 5-8 and Example 1 is that the amounts of silicon nitride and sintering aids are different from those in Example 1. The differences are shown in Table 1.

[0038] Table 1. Raw material usage and proportions for Examples 1-8 Example 9 The difference between Example 9 and Example 1 is that, in step S4, the method for preparing the joint prosthesis component by mixing powders includes the following steps: 1) The mixed powder is cold isostatically pressed under a pressure of 230 MPa to obtain a blank; 2) The blank material is machined to obtain the joint prosthesis component.

[0039] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the sintering aid is only yttrium oxide.

[0040] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the sintering aid is only magnesium oxide.

[0041] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the sintering aid is only alumina.

[0042] Experimental testing Experimental tests were conducted on Examples 1-8 and Comparative Examples 1-3, and the test results are shown in Table 2.

[0043] Table 2. Experimental results of Examples 1-8 and Comparative Examples 1-3 Examples 10-13 The difference between Examples 10-13 and Example 1 is that the particle size of the mixed powder in step S3 is different. See Table 3 for the differences.

[0044] Table 3. Particle size of the mixed powders from Examples 1 and 10-13 Experimental testing Experimental tests were conducted on Examples 10-13 and Example 1, and the test results are shown in Table 4.

[0045] Table 4. Experimental test results of Examples 10-13 and Example 1 Examples 14-17 The difference between Examples 14-17 and Example 1 is that the temperature and pressure of vacuum hot pressing sintering in step S5 are different. See Table 5 for the differences.

[0046] Table 5. Temperature and pressure of vacuum hot pressing sintering in Examples 1 and 14-17 Temperature (°C) Pressure (MPa) Example 1 1500 30 Example 14 1300 35 Example 15 1800 25 Example 16 1900 25 Example 17 1200 35 Experimental testing Experimental tests were conducted on Examples 14-17 and Example 1, and the test results are shown in Table 6.

[0047] Table 6. Experimental test results of Examples 14-17 and Example 1. Examples 18-22 The difference between Examples 18-22 and Example 1 is that the coating thickness formed by vacuum plasma spraying is different, and the differences are shown in Table 7.

[0048] Table 7 Coating thickness in step 5 of Examples 1 and 18-22 Coating thickness (mm) Example 1 1 Example 18 0.1 Example 19 0.25 Example 20 0.75 Example 21 1.5 Example 22 1.75 Experimental testing Experimental tests were conducted on Examples 18-22 and Example 1, and the test results are shown in Table 8.

[0049] Table 8. Experimental test results of Examples 18-22 and Example 1 Results Analysis As can be seen from Examples 1-9, Comparative Examples 1-3, and Tables 1 and 2, the joint prosthesis components prepared using the raw material composition and proportion of this application and according to the preparation process of this application have better performance.

[0050] Based on Examples 1, 10-13, and Tables 3 and 4, it can be seen that the particle size of the mixed powder in step S3 affects the performance of the obtained joint prosthesis. When the particle size of the mixed powder is 200-300 mesh, the joint prosthesis has better performance.

[0051] Based on Examples 1, 14-17, and Tables 5 and 6, it can be seen that when the temperature of vacuum hot pressing sintering in step S5 is 1300-1800℃ and the pressure is 25-35MPa, the joint prosthesis component produced has better performance.

[0052] Based on Examples 1, 18-22, and Tables 7 and 8, it can be seen that the coating thickness formed by vacuum plasma spraying in step S5 has a significant impact on the wear resistance of the joint prosthesis. When the coating thickness is too large, the wear resistance of the joint prosthesis decreases. When the coating thickness is 0.25-1.5 mm, the wear resistance of the joint prosthesis is better.

[0053] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A manufacturing process for a non-metallic self-lubricating joint prosthesis component, characterized in that, Includes the following steps: S1. Weigh and mix silicon nitride and sintering aid to obtain a mixture; S2. The mixture obtained in step S1 is added to an ethanol solution with a mass fraction of 75-85% and ultrasonically dispersed to obtain a dispersion. The pH of the dispersion is adjusted to 5-6 with acetic acid. S3. After heating the dispersion obtained in step S2 to 70-80℃ and stirring for 6-8 hours, centrifuge to obtain precipitate, then vacuum dry the precipitate and pulverize it to obtain mixed powder. S4. Use the mixed powder obtained in step S3 to prepare the joint prosthesis component; S5. The joint prosthesis component obtained in step S4 is subjected to vacuum hot pressing sintering, and the sintered joint component is polished. Then, the surface of the joint prosthesis component is subjected to vacuum plasma spraying to form a coating, thereby obtaining the non-metallic self-lubricating joint prosthesis component. In step S5, the spraying material for vacuum plasma spraying is one of titanium, titanium + HA, or pure tantalum, and the resulting coating thickness is 0.25~1.5mm.

2. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S1, 80-90 parts of silicon nitride and 10-20 parts of sintering aid are weighed out by weight.

3. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, The sintering aids include yttrium oxide, aluminum oxide and magnesium oxide, and the mass ratio of yttrium oxide, aluminum oxide and magnesium oxide is (3-6):(2-5):(2-5).

4. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S2, the ultrasonic frequency is 55-65kHz and the ultrasonic dispersion time is 20-30min.

5. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S3, the particle size of the mixed powder is 200-300 mesh.

6. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S4, the method for preparing the joint prosthesis component by mixing powder includes the following steps: 1) The mixed powder is cold isostatically pressed to obtain a blank; 2) The blank material is machined to obtain the joint prosthesis component.

7. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S4, the method for preparing the joint prosthesis component by mixing powder is 3D printing.

8. The manufacturing process of the non-metallic self-lubricating joint prosthesis component according to claim 1, characterized in that, In step S5, the temperature of vacuum hot pressing sintering is 1300-1800℃ and the pressure is 25-35MPa.

9. A non-metallic self-lubricating joint prosthesis component prepared by the manufacturing process of any one of claims 1-8.

Citation Information

Patent Citations

  • Biomedical silicon nitride composition and method for preparing silicon nitride ceramics

    CN109467441A

  • Methods and compositions for creating an atomic composite of ceramics coated with titanium making use of coating methodology

    WO2009103775A2