A MOF membrane for efficient separation of C6 alkane isomers and a preparation method thereof

By preparing Al-bttotb MOF membranes, using support pretreatment and modification to form strong bonds, and combining growth regulators to promote MOF membrane nucleation, the problem of low separation efficiency of C6 alkane isomers was solved, achieving efficient and low-energy separation and improving the octane number.

CN117654317BActive Publication Date: 2026-11-24PETROCHINA CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211019166.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-24
Publication Date
2026-11-24
Estimated Expiration
2042-08-24

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently separate C6 alkane isomers, especially straight-chain alkanes from single- and double-branched isomers, limiting octane number enhancement. Furthermore, traditional methods are energy-intensive and complex.

Method used

The Al-bttotb MOF membrane preparation method involves pretreating and modifying a porous alumina support, using organic ligands to form strong bonds with aluminum atoms on the support surface, and combining growth regulators to promote the nucleation and growth of the MOF membrane, forming a dense MOF membrane, which is then used for separation by utilizing its unique pore structure.

Benefits of technology

It achieves efficient separation of C6 alkane isomers at room temperature and pressure, improves octane number, reduces energy consumption, and the MOF membrane has high bonding strength with the support, exhibiting excellent thermal and chemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117654317B_ABST
    Figure CN117654317B_ABST
Patent Text Reader

Abstract

This invention provides a MOF membrane for efficient separation of C6 alkane isomers and its preparation method. The one-dimensional pore size of the MOF structure of the MOF membrane is the same as that of the MOF membrane for efficient separation of C6 alkane isomers provided by this invention. The pore size of the MOF structure is between the molecular dynamic diameters of mono- and di-branched hexanes, which can play the role of sieving mono- and di-branched hexanes and can effectively separate C6 mono- and di-branched alkanes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of membrane separation technology, specifically to a MOF membrane for efficient separation of C6 alkane isomers and its preparation method. Background Technology

[0002] Light naphtha is mainly composed of alkane isomers, which undergo catalytic isomerization to produce isomers with different degrees of branching. These alkane isomers can be used as valuable gasoline blending components. Generally, more branched alkanes have higher octane numbers (RON) than less branched isomers. To ensure the production of gasoline with high RON, it is necessary to remove alkane isomers with low RON from the mixture and recycle them back to the catalytic reactor. This means removing straight-chain alkanes, or ideally, separating straight-chain and monobranched alkanes from the dibranched isomers, which have the highest octane numbers and are high-quality gasoline blending components. However, because alkane isomers have similar chemical and physical properties, separating alkane isomers with different degrees of branching is a key but challenging process for improving octane numbers in the petrochemical industry.

[0003] Separation via traditional distillation is not only difficult but also energy-intensive, while adsorption separation technology is an economical and effective method that can achieve the adsorption separation of alkane isomers under mild conditions. For example, zeolite 5A (Industrial & Engineering Chemistry Research, 2012, 51(12):4692-4702.) is the only adsorbent used industrially to date for separating alkane isomers. However, zeolite 5A adsorption separation has not been widely used as a substitute for distillation, and is only used sporadically as a supplement in some refineries. This is because the separation performance of zeolite 5A cannot fully meet the requirements of industrial processes. Furthermore, the low adsorption capacity of zeolite 5A limits its separation efficiency. More importantly, its inability to adsorb any branched alkanes hinders its ability to further improve the octane number by distinguishing between monobranched and dibranched isomers. While Fe2(BDP)3 (Science, 2013, 340(6135): 960-964.) can thermodynamically distinguish monobranched and dibranched alkane isomers, this separation based on the difference in affinity between the adsorbate and the framework through free diffusion results in relatively low selectivity. Ca-tcpb (Energy & Environmental Science, 2018, 11(5): 1226-1231.) can separate ternary mixtures of linear, monobranched, and dibranched alkanes into pure components using programmed temperature rise due to its structural flexibility. Although ideal size exclusion-based separation is achieved, it is limited to specific temperatures and pressures, which is not practical for the naphtha industry.

[0004] Adsorption separation suffers from high desorbent consumption, difficult regeneration, and complex processes in practice, requiring further improvement. Compared to distillation and adsorption separation, membrane separation technology is an emerging chemical separation technology that is environmentally friendly, efficient, and produces less pollution. For example, the ZSM-5 membrane (Journal of Membrane Science, 2000, 176(1):43-53.) exhibits good separation performance for the hexane / 2,2-dimethylbutane mixed system. At 390 K, the selectivity of hexane / 2,2-dimethylbutane is 35%, and the permeation rate of hexane is 2.5 × 10⁻⁵. -3 mol m-2·s -1 However, like zeolite 5A, they cannot separate single-branched and dibranched isomers. While the Zeolite Beta membrane (Microporous Mesoporous Mater, 2010, 128(1-3): 194-202.) can separate 3-methylpentane and 2,2-dimethylbutane, its selectivity at 443 K is only 1.46, indicating poor separation performance. Furthermore, the feed conditions require heating, increasing energy consumption and operational complexity.

[0005] In recent years, metal-organic frameworks (MOFs) have become particularly suitable as materials for industrially challenging separations due to their advantages such as permanent porosity, high stability, tunable pore size, and ease of functionalization. Traditional in-situ synthesis methods for preparing MOF membranes mostly involve direct growth of the MOF membrane on the support without any pretreatment. While this method is relatively simple and highly reproducible, heterogeneous nucleation is unfavorable for membrane growth, resulting in weak interactions between the support and the MOF. Consequently, the prepared membrane material is prone to detachment, making it difficult to form large-area, continuous, and dense membranes. To improve the interaction between the support and the MOF, most existing techniques involve pretreatment or modification of the support.

[0006] Chinese patent document CN109721737A discloses a method for preparing a hybrid material containing a metal-organic framework (MOF) for the selective adsorption separation of ethylene / ethane and propylene / propane. The disclosed technical solution first immerses the support in an organic ligand solution, then transfers the material to a reactor containing a copper salt solution. This is to employ low-temperature nucleation-induced migration technology to promote the migration of the MOF prepolymer into the aluminosilicate support plate, ensuring uniform growth of the MOF on both the inner and outer surfaces of the aluminosilicate plate, shortening the crystal nucleation time, and resulting in uniform crystal size of the MOF material itself. The processing method does not involve heating after ligand immersion; instead, heating is performed after the formation of the MOF prepolymer (organic ligand and metal salt) within the support. This material separates olefins and alkanes through adsorption separation. However, the structure in the patent exhibits poor adsorption separation efficiency for alkane isomers, and due to the weak interaction between the MOF grains and the support, a dense MOF film cannot be formed. Summary of the Invention

[0007] The purpose of this invention is to provide a MOF membrane for efficient separation of C6 alkane isomers and its preparation method, so as to overcome the defects of existing MOF membranes such as poor separation effect of alkane isomers.

[0008] To achieve the above objectives, this invention provides a MOF membrane for the efficient separation of C6 alkane isomers, wherein the one-dimensional pore size of the MOF structure is [missing information]. It lies between the molecular dynamic diameters of single- and dibranched hexanes, and can be used to screen single- and dibranched hexanes.

[0009] The MOF membrane is an Al-bttotb membrane, where bttotb represents H3bttotb, which is an abbreviation for 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid.

[0010] The present invention also provides a method for preparing the above-mentioned MOF membrane for efficient separation of C6 alkane isomers, comprising the following steps:

[0011] Carrier pretreatment: The surface of the sheet-like porous alumina carrier is polished, cleaned and dried to obtain the pretreated alumina carrier;

[0012] Carrier modification: 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is dissolved in a solvent to obtain a modification mixture; then the pretreated alumina carrier is vertically placed into the modification mixture, heated at 180-250°C, removed, rinsed, and dried to obtain the modified alumina carrier.

[0013] Film formation: The metal precursor and 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid are dissolved in a solvent, and a growth regulator is added to obtain the synthesis solution of MOF; then the modified alumina support is vertically placed into the synthesis solution of MOF and heated at 150-180°C to obtain the MOF film.

[0014] The method for preparing MOF membranes provided by this invention involves first immersing a sheet-like porous alumina support in a specific 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid solution (modification mixture), and then heating to allow the 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid and the support to form a bond. Specifically, this bond is formed between the Al atoms in the support and the O atoms in the metal-organic ligands, which is similar to the Al-O bond in the metal-organic framework structure. This allows the ligands to adhere firmly to the support, and during the subsequent crystallization process, the ligands attached to the surface of the support can become part of the metal-organic framework, thereby forming a strong and dense Al-bttotb membrane. Adding a growth regulator to the MOF synthesis solution helps to improve the grain morphology of the membrane surface and improve the membrane quality.

[0015] Optionally, the heating time in the carrier modification step is 12–24 hours. By limiting the heating time in the carrier modification step, porous alumina carriers with different crystal coverage can be obtained, while Al-O bonds are formed between the organic ligand and the carrier.

[0016] Optionally, the heating time in the film-forming step is 2 to 7 days.

[0017] Optionally, in the carrier modification, the molar ratio of the solvent to the 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is 100:1 to 200:1.

[0018] Optionally, in the synthesis solution of the MOF, the molar ratio of the 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid to the metal ions in the metal precursor is 1:1 to 10:1, preferably 5:1 to 8:1; the molar ratio of the solvent to the 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is 200:1 to 600:1; and the molar ratio of the growth regulator to the 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is 50:1 to 380:1.

[0019] Optionally, in the carrier modification step and film formation, the solvent is selected from one or more combinations of methanol, ethanol, water and N,N-dimethylformamide;

[0020] The growth regulator is selected from formic acid.

[0021] Optionally, in the carrier pretreatment step, the sheet-like porous alumina carrier has a thickness of 1-5 mm, a diameter of 18-25 mm, an average pore size of 80-150 nm, and a porosity of 20%-60%.

[0022] Optionally, in the film-forming step, the metal precursor is selected from any one of aluminum nitrate nonahydrate, aluminum sulfate, and aluminum chloride hexahydrate.

[0023] Optionally, the preparation method of the MOF membrane for efficient separation of C6 alkane isomers further includes an activation step: immersing the MOF membrane obtained in the film formation step in a solvent and drying it, preferably for 12-24 hours, at a temperature of 50-80°C, for 12-24 hours.

[0024] Optionally, the solvent used in the activation step is selected from one or more combinations of methanol, ethanol, water, and N,N-dimethylformamide.

[0025] Optionally, the carrier modification step further includes adding a growth regulator to the modification mixture. Preferably, the growth regulator is selected from formic acid; more preferably, the molar ratio of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid to the growth regulator is 0.006:1 to 0.012:1. By adding a growth regulator to the modification mixture, the ligand can be firmly and uniformly attached to the carrier.

[0026] Optionally, in the carrier pretreatment step, the sheet-like porous alumina carrier is prepared by pressing and sintering several sheets of porous alumina.

[0027] Specifically, the carrier pretreatment step is as follows: the sheet-like porous alumina carrier is polished with sandpaper, then cleaned with ethanol and deionized water in sequence, and dried in a muffle furnace at 400-500℃ for 10-16 hours; thus, the pretreated alumina carrier is obtained.

[0028] This invention does not limit the types and proportions of C6 alkane isomers, such as combinations of two or more of n-hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane and 2,3-dimethylbutane.

[0029] To achieve the above objectives, the present invention also provides a method for separating C6 alkane isomers, wherein the above-mentioned MOF membrane is used to pass a mixture of C6 alkane isomers through the MOF membrane at room temperature and pressure using a pervaporation device. The MOF membrane allows straight-chain alkanes and monobranched isoalkanes to pass through, while excluding dibranched isoalkanes.

[0030] Specifically, under normal temperature and pressure, the prepared C6 alkane isomer mixture is placed in a feed tank, and the feed liquid is pumped into the pervaporation membrane module. Because the permeate side is maintained under vacuum by a vacuum pump, a vapor pressure difference exists across the MOF membrane. This pressure difference drives the feed liquid into the membrane and then permeates downstream into the permeate section. The MOF membrane exhibits selective permeation, resulting in the permeate downstream being predominantly composed of n-hexane and 3-methylpentane. The permeate components are then piped into a permeate vapor condenser, where the permeate product vapor is collected under liquid nitrogen. The composition of the feed and permeate is measured using a gas chromatograph. The retained liquid that does not permeate the membrane is recycled back into the feed liquid. Preferably, the pervaporation process operates at a temperature of 25°C and a feed-side pressure of 0 MPa.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0032] 1. The MOF membrane for efficient separation of C6 alkane isomers provided by this invention has a MOF structure with a pore size of [missing information]. Its pore size is between the molecular dynamic diameters of single- and dibranched hexanes, which can be used to screen single- and dibranched hexanes and effectively separate C6 single- and dibranched alkanes.

[0033] 2. This invention modifies a porous alumina support with organic ligand compounds at a specific temperature of 180–250°C. This allows the organic ligands to react with aluminum atoms in the support and attach to the support surface, providing abundant adhesion sites for MOF nucleation. This facilitates the formation of a continuous and dense MOF film, lowers the energy barrier required for crystal nucleation on the support surface, and reduces the difficulty of nucleation. Simultaneously, it overcomes the problem of competing bulk nucleation processes in the reaction solution reducing the number of surface nuclei. Combined with subsequent film-forming steps, heating at 150–180°C allows the organic ligands bonded to the support surface to attract more metal ions from the MOF synthesis solution for coordination, promoting grain nucleation on the support surface and ultimately growing into a dense MOF film. The continuous and dense MOF film obtained by this method has a higher bonding strength with the support and is less prone to detachment in subsequent testing. Even under heating conditions of 125°C, it maintains the stability of the framework, exhibiting excellent thermal stability. Furthermore, after immersion in a C6 mixture for 20 hours, no framework collapse was observed, demonstrating excellent chemical stability.

[0034] 3. The MOF membrane preparation method of the present invention is simple, has excellent thermal and chemical stability, and most importantly, its unique pore structure only allows straight-chain alkanes and single-branched isoalkanes to pass through, excludes double-branched isoalkanes, and the feeding conditions are at room temperature and pressure, which reduces energy consumption in the operation process and can be recycled.

[0035] 4. In the process of separating C6 alkane isomers, this invention utilizes the differences in adsorption-diffusion rates and molecular size of the components in the membrane pores, driven by the vapor pressure difference of the components. That is, through the adsorption-diffusion and molecular sieving effects of the membrane, n-hexane and 3-methylpentane are preferentially permeated. Furthermore, the mass fraction of n-hexane and 3-methylpentane is concentrated from 67% on the feed side to 87% on the permeate side, while 2,2-dimethylbutane decreases from 33% to 13%. It is not limited by the gas-liquid balance of the separation system, has high separation efficiency, and is suitable for the separation of azeotropic and near-boiling mixtures. Attached Figure Description

[0036] Figure 1a This is a surface SEM image of the modified porous alumina support in Example 1 of the present invention after heating in a modified mixture at 200°C for 12 hours;

[0037] Figure 1b This is a surface SEM image of the modified porous alumina support in Example 1 of the present invention after heating in a modified mixture at 200°C for 18 hours;

[0038] Figure 1c This is a surface SEM image of the modified porous alumina support in Example 1 of the present invention after heating in a modified mixture at 200°C for 24 hours;

[0039] Figure 1d The images show the XRD patterns of the modified porous alumina support in Example 1 of this invention after heating in the modified mixture at 200°C for 12h, 18h, and 24h (☆ in the images represent the characteristic peaks of the porous alumina support).

[0040] Figure 2a This is a surface SEM image of the Al-bttotb film prepared in Example 1 of this invention;

[0041] Figure 2b This is a cross-sectional SEM image of the Al-bttotb film prepared in Example 1 of this invention;

[0042] Figure 2c This is the XRD pattern of the Al-bttotb membrane prepared in Example 1 of the present invention (☆ in the figure represents the characteristic peak of the porous alumina support);

[0043] Figure 3 This is the functional relationship between the permeability and the diameter of the kinetic gas when a single-component gas passes through the Al-bttotb membrane prepared in Example 1 in this invention;

[0044] Figure 4a This invention relates to the relationship between the separation performance of the H2 / C3H8 mixture (volume ratio of 50:50) and temperature when separated by an Al-bttotb membrane prepared in Example 1.

[0045] Figure 4b This invention relates the separation performance of the H2 / C3H8 mixture (volume ratio 50:50) obtained by using an Al-bttotb membrane prepared in Example 1 to the immersion time in the C6 alkane isomer mixture.

[0046] Figure 5 This is a graph showing the performance of the Al-bttotb membrane obtained in Example 1 of this invention in separating a mixture of ternary C6 alkane isomers with equal mass fractions.

[0047] Figure 6 This is a surface SEM image of the Al-bttotb film prepared by in-situ synthesis in Comparative Example 1 of this invention. Detailed Implementation

[0048] The present invention will now be described in detail through embodiments. It should be noted that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above description.

[0049] The efficient separation of C6 alkane isomers is crucial for the low-carbon transformation of refining processes. Improving the separation selectivity of light naphtha can yield high-octane gasoline, achieving a low-carbon transition in refining. Traditional separation methods involve 5A molecular sieve adsorption, which can only separate normal-isomerized alkanes, resulting in low octane numbers in the adsorbed oil. Simulated moving bed adsorption requires significant energy consumption for desorption. Employing single- and double-branched alkane membrane separation technology could improve the octane number of the adsorbed oil and significantly reduce energy consumption by eliminating the need for desorption. However, existing MOF membranes exhibit poor separation performance for C6 alkane isomers. Research has revealed that this is because the pore structure and chemical environment of existing MOF membranes lack specificity for various C6 alkane isomers, leading to poor separation efficiency. Therefore, constructing MOF membranes with suitable structures, chemical environments, and pores, while also possessing excellent stability and ease of preparation, based on the molecular characteristics of C6 alkane isomers, is a pressing problem to be solved.

[0050] Through further in-depth research, the inventors discovered that the one-dimensional pore size of the MOF structure is... Located between the molecular dynamic diameters of single- and dibranched hexanes, it can be used for sieving single- and dibranched hexanes, exhibiting excellent separation performance. Especially when the MOF is Al-bttotb, the Al-O bond formed is more stable due to the trivalent oxidation state of Al, resulting in higher stability.

[0051] In one embodiment, the present invention also provides a method for preparing the above-mentioned MOF membrane, comprising:

[0052] Carrier pretreatment: Several sheet-like porous alumina carriers manufactured by pressing and sintering are polished with sandpaper. The resulting alumina carriers are cleaned with ethanol and deionized water respectively, and dried in a muffle furnace at 400-500℃ for 10-16 hours to obtain pretreated alumina carriers.

[0053] Support modification: 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in a solvent to prepare a modification mixture. The pretreated porous alumina support was vertically placed into the modification mixture and heated at 180–250°C. The porous alumina support was then removed, rinsed, and dried, allowing the organic ligands to react with the aluminum atoms of the support and attach to the support surface, resulting in the modified porous alumina support. The support modification step allows the ligands to form a stronger bond with the support before the film, providing more attachment sites for the growth of MOF grains during the subsequent film formation process, thus obtaining a dense film.

[0054] Film formation: The metal precursor salt, 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid and growth regulator were dissolved in a solvent to prepare the MOF synthesis solution. The modified porous alumina support was vertically placed into a reactor containing the MOF synthesis solution and heated at 150-180°C. The organic ligands bonded to the support surface attracted more metal ions from the MOF synthesis solution to coordinate with it, promoting the nucleation of grains on the support surface and eventually growing into a dense MOF film.

[0055] This invention first utilizes the bonding and reaction between aluminum atoms on a porous alumina support and oxygen atoms in 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid at high temperature, thereby providing abundant attachment sites for MOF nucleation. This facilitates the formation of a continuous and dense MOF film, reduces the high energy barrier that the nucleation process on the support surface must overcome, and solves the problem of high nucleation difficulty. At the same time, it overcomes the problem of competing bulk nucleation processes in the reaction solution reducing the number of crystal nuclei on the surface. Then, by reacting the modified porous alumina support with the MOF synthesis solution at 150-180°C, the growth of MOF crystals can be well controlled, resulting in MOF films with suitable structure, chemical environment, and pore structure for various C6 alkane isomers.

[0056] Furthermore, compared with the traditional in-situ synthesis method, the MOF membrane prepared by the present invention is continuous and dense due to the formation of a large number of nucleation sites, and the MOF membrane has a higher binding strength with the support, exhibiting excellent thermal stability, long-range stability and chemical stability. At the same time, it can be used for the efficient separation of C6 alkane isomers and has broad application prospects.

[0057] Preferably, in one embodiment, in the carrier pretreatment step, the porous alumina carrier has a thickness of 1-5 mm, a diameter of 18-25 mm, an average pore size of 80-150 nm, and a porosity of 20%-60%.

[0058] Preferably, in one embodiment, in the support modification step, the solvent is selected from one or more combinations of methanol, ethanol, water and DMF, and the heating time is preferably 12 to 24 hours to obtain porous alumina supports with different crystal coverage, and Al-O bonds are formed between the organic ligand and the support.

[0059] Preferably, in one embodiment, in the film-forming step, the metal precursor salt is selected from any one of aluminum nitrate nonahydrate, aluminum sulfate, and aluminum chloride hexahydrate; the solvent is selected from one or more combinations of methanol, ethanol, water, and DMF.

[0060] Preferably, in one embodiment, the molar ratio of solvent to 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid in the modified mixture is 100:1 to 200:1.

[0061] Preferably, in one embodiment, in the MOF synthesis solution, the molar ratio of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid to the metal ions in the metal precursor salt is 1:1 to 10:1, the molar ratio of solvent to 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is 200:1 to 600:1, and the molar ratio of growth regulator to 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid is 50:1 to 380:1.

[0062] Preferably, in one embodiment, the method further includes an activation step of the prepared MOF: the MOF membrane obtained in the film-forming step is immersed in a solvent at room temperature for 12-24 hours, and then taken out and dried at 50-80°C for 12-24 hours.

[0063] The MOF membrane preparation method provided by this invention, through a further activation step, combined with the aforementioned support pretreatment, support modification and film formation steps, with each step working together, can further promote the bonding reaction between the organic ligand 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid and the porous alumina support, providing nucleation sites for the subsequent growth of MOF membrane, further improving the compactness of MOF membrane and reducing its continuity and defect-free nature.

[0064] The MOF membrane provided by this invention is used for the efficient separation of C6 alkane isomers. The membrane separation method can be a conventional method, such as: at room temperature and pressure, a mixture of C6 alkane isomers is passed through the MOF membrane using a pervaporation device. Due to the unique pore structure of the MOF membrane, straight-chain alkanes and monobranched isoalkanes can pass through, while dibranched isoalkanes are excluded, thus achieving efficient separation of alkane isomers.

[0065] This invention does not impose any particular limitation on the types and proportions of C6 alkane isomers. The C6 alkane isomers are selected from two or more combinations of n-hexane, 2-methylpentane, 3-methylpentane, 2,2-dimethylbutane, and 2,3-dimethylbutane. For example, the mass ratio of n-hexane to 2,2-dimethylbutane is 1:99 to 99:1. The pervaporation process is operated at a temperature of 25°C and the feed-side pressure is 0 MPa.

[0066] In a preferred embodiment, the organic ligand of the MOF membrane material of the present invention is 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid, and the metal ion in the metal precursor salt is Al. 3+ Formic acid was used as the growth regulator. Hexane, 3-methylpentane, and 2,2-dimethylbutane (mass ratio 1:1:1) were separated under ambient temperature and pressure. The MOF membrane preferentially permeated with hexane and 3-methylpentane, and the total mass fraction of hexane and 3-methylpentane increased from 67% on the feed side to 87% on the permeate side, while the 2,2-dimethylbutane content decreased from 33% to 13%.

[0067] Therefore, the MOF membrane provided by this invention is used for the separation of C6 alkane isomers. Compared with distillation and solid adsorption, it has the advantages of mild operating conditions, low equipment investment, energy saving and environmental protection, low energy consumption and low cost, and has significant prospects for industrial application. At the same time, the MOF membrane preparation method provided by this invention has the advantages of simplicity, high thermal and chemical stability, and easy scale-up.

[0068] The technical solution of the present invention will be further described in detail below through specific embodiments. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0069] Example 1

[0070] Carrier pretreatment: The sheet-like porous alumina carrier (thickness 5 mm, diameter 20 mm, average pore size 100 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0071] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain a modified alumina carrier mixture. The dried alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified alumina mixture using tweezers and reacted in an oven at 200 °C for 12 h, 18 h, and 24 h, respectively, to obtain porous alumina carriers with different crystal coverage. After the reaction, the modified alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0072] The modified alumina support prepared above was subjected to SEM and XRD tests, respectively. Figure 1a , Figure 1b , Figure 1c These are SEM images of the modified porous alumina supports prepared at different reaction times. Figure 1d These are XRD patterns of the modified porous alumina supports prepared at different reaction times. Figure 1a , Figure 1b and Figure 1c The comparison shows that Al-bttotb crystals appear on the surface of the porous alumina support, and the crystal coverage on the support surface becomes increasingly dense with increasing reaction time. Figure 1d It can be seen that as the reaction time increases, the characteristic diffraction peak (8.72°) of Al-bttotb crystal also gradually increases.

[0073] Film formation: 0.15 g of aluminum nitrate nonahydrate and 0.35 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support (the modified porous alumina support with the best crystal coverage obtained by reacting in an oven at 200 °C for 24 h) was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 150 °C for 3 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0074] Figure 2a and Figure 2b These are SEM images of the surface and cross-section of the Al-bttotb film, respectively. Figure 2a It can be seen that the surface of the membrane is uniform, without visible cracks, pinholes or other defects. Figure 2b It can be seen that the Al-bttotb membrane has excellent symbiotic properties and a thickness of about 8 μm. This continuous top film grows densely and adheres firmly to the top of the porous alumina support. Figure 2c The XRD pattern of the Al-bttotb film is shown below. Figure 2c It can be seen that the characteristic peaks of this Al-bttotb film match well with the published XRD patterns of Al-bttotb crystals. Figure 2c The three asterisked peaks (25.52°, 35.08°, and 37.72°) after 25° are peaks of the alumina support, while the XRD pattern of Al-bttotb crystal only shows the peaks of Al-bttotb, so it does not have the three asterisked peaks after 25°.

[0075] After the membrane was removed from the reactor during the above film-forming process, Al-bttotb powder crystals were also found in the remaining liquid. The most probable pore size of the Al-bttotb powder crystals obtained after filtration was determined using the BET micropore testing method under the DFT model. Since the Al-bttotb structure contains only one-dimensional channels, the most probable pore size can be measured as equivalent to the pore size of its one-dimensional channels.

[0076] The Al-bttotb membrane prepared above was subjected to single-component gas permeability tests for H2, CO2, N2, CH4, C2H6, C3H8 and i-C4H8, with a gas flow rate of 40 mL / min. Figure 3This is the functional relationship between the permeability of a single-component gas passing through the aforementioned Al-bttotb membrane and the kinetic gas diameter, derived from... Figure 3 It is known that the permeability of hydrogen through the Al-bttotb membrane is much higher than that of other gases, and the permeability decreases sharply with the increase of the diameter of the kinetic gas, exhibiting a significant molecular sieving effect. The theoretical selectivity of H2 / CO2, H2 / N2, H2 / CH4, H2 / C2H6, H2 / C3H8, and H2 / i-C4H8 are 5.0, 4.3, 4.7, 17.2, 38.3, and 76.6, respectively, all higher than their corresponding Knudsen selectivity of 4.7, 3.7, 2.8, 3.9, 4.7, and 5.3, indicating that the Al-bttotb membrane provided by this invention has good compactness.

[0077] The Al-bttotb films prepared above were subjected to thermal stability and chemical stability tests, respectively. Figure 4a and Figure 4b The figures show the separation performance of an H2 / C3H8 mixture (volume ratio 50:50) on an Al-bttotb membrane in relation to temperature and immersion time in a C6 mixture, with a total gas flow rate of 40 mL / min. Figure 4a It can be seen that when the temperature rises from 25℃ to 125℃ at a heating rate of 5℃ / min, the selectivity of H2 / C3H8 is not affected. Furthermore, when the temperature returns to 25℃, the gas flux and selectivity return to their initial values, indicating that the Al-bttotb membrane possesses excellent thermal stability. Figure 4b It can be seen that when the Al-bttotb membrane is immersed in a membrane module containing a mixture of C6 alkane isomers, the gas flux and selectivity of the Al-bttotb membrane decrease slightly with increasing time. After removing the organic matter on the membrane surface by drying at 80℃ for 24 hours, the flux and selectivity are close to the initial values, indicating that the Al-bttotb membrane has good solvent resistance.

[0078] The Al-bttotb membrane prepared above was subjected to pervaporation testing. The process included the following steps: a mixture of C6 alkane isomers (equal mass fractions of n-hexane, 3-methylpentane, and 2,2-dimethylbutane (1:1:1)) was added to a feed liquid tank. At ambient temperature and pressure, the C6 alkane isomer mixture was pumped into the pervaporation membrane module. Because the permeate side was maintained under vacuum by a vacuum pump, a vapor pressure difference existed across the Al-bttotb membrane. This pressure difference propelled the feed liquid into the Al-bttotb membrane, which then permeated downstream into the permeate section. The Al-bttotb membrane exhibits selective permeation, resulting in the downstream permeate being predominantly composed of n-hexane and 3-methylpentane. The permeate was then fed into a permeate vapor condenser, where the permeate vapor was collected under liquid nitrogen. The composition of the feed and permeate was measured using a gas chromatograph. The retained liquid that did not permeate the membrane was recycled back to the feed liquid.

[0079] Figure 5 This is a performance graph of an Al-bttotb membrane separating a mixture of ternary C6 alkane isomers with equal mass fractions. Figure 5 It can be seen that the Al-bttotb membrane preferentially permeates n-hexane and 3-methylpentane, and the total mass fraction of n-hexane and 3-methylpentane is concentrated from 67% on the feed side to 87% on the permeate side, while the mass fraction of 2,2-dimethylbutane decreases from 33% on the feed side to 13% on the permeate side.

[0080] Comparative Example 1

[0081] Carrier pretreatment: The sheet-like porous alumina carrier (5 mm, diameter 20 mm, average pore size 100 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0082] Film formation: 0.15 g of aluminum nitrate nonahydrate and 0.35 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The pretreated porous alumina support was then vertically placed into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and placed in an oven at 150 °C for 3 days. After the reaction was completed, the mixture was cooled to room temperature, the membrane was removed and gently washed in DMF, and then immersed in fresh anhydrous methanol for 12 h for activation. Finally, the membrane was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0083] The Al-bttotb film described above was subjected to SEM testing, as follows: Figure 6 As shown, by Figure 6 It can be seen that the Al-bttotb film has obvious defects, exposing a large area of ​​alumina support, indicating that it does not have continuous compactness.

[0084] Comparative Example 2

[0085] Carrier pretreatment: The sheet-like porous alumina carrier (thickness 5 mm, diameter 20 mm, average pore size 100 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0086] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The dried alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 200 °C for 24 h. After the reaction, the modified alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0087] Film formation: 0.12 g of zinc nitrate hexahydrate and 0.35 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 150 °C for 3 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Zn-bttotb membrane.

[0088] The Zn-bttotb membrane obtained in Comparative Example 2 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0089] Comparative Example 3

[0090] Carrier pretreatment: The sheet-like porous alumina carrier (thickness 5 mm, diameter 20 mm, average pore size 100 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0091] Carrier modification: 0.27 g of terephthalic acid was dissolved in 20 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The dried alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 200 °C for 24 h. After the reaction, the modified alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0092] Film formation: 0.15 g of aluminum nitrate nonahydrate and 0.12 g of terephthalic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and placed in an oven at 150 °C for 3 days. After the reaction was completed, the mixture was cooled to room temperature. The membrane was removed and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bdc membrane.

[0093] After the membrane was removed from the reactor during the above film-forming process, Al-bdc powder crystals were also found in the remaining liquid. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0094] The performance of the Al-bdc membrane obtained in Example 3 was tested using the same method as in Example 1.

[0095] Example 2

[0096] Carrier pretreatment: The sheet-like porous alumina carrier (1 mm, diameter 18 mm, average pore size 80 nm; porosity 40%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0097] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 24.5 mL of LDMF, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 180 °C for 20 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0098] Film formation: 0.134 g of aluminum sulfate and 0.35 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then vertically placed into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 180 °C for 2 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0099] After the membrane was removed from the reactor during the above film-forming process, Al-bttotb powder crystals were also found in the remaining liquid. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0100] The Al-bttotb membrane obtained in Example 2 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0101] Example 3

[0102] Carrier pretreatment: The sheet-like porous alumina carrier (4 mm, diameter 25 mm, average pore size 150 nm; porosity 40%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0103] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 12.5 mL of LDMF, and 5 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers, and reacted in an oven at 250 °C for 18 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0104] Film formation: 0.97 g of aluminum nitrate nonahydrate and 1.26 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 5 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then vertically placed into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and placed in an oven at 180 °C for 3 days. After the reaction was completed, the mixture was cooled to room temperature, the membrane was removed and gently washed in DMF, and then immersed in fresh anhydrous methanol for 12 h for activation. Finally, the membrane was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0105] Al-bttotb powder crystals were also present in the liquid of the reactor during the above film formation process. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0106] The Al-bttotb membrane obtained in Example 3 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0107] Example 4

[0108] Carrier pretreatment: The sheet-like porous alumina carrier (4 mm, diameter 24 mm, average pore size 120 nm; porosity 60%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0109] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 220 °C for 19 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0110] Film formation: 0.23 g of aluminum nitrate nonahydrate and 0.84 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 170 °C for 4 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0111] Al-bttotb powder crystals were also present in the liquid of the reactor during the above film formation process. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0112] The Al-bttotb membrane obtained in Example 4 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0113] Comparative Example 4

[0114] Carrier pretreatment: The sheet-like porous alumina carrier (4 mm, diameter 24 mm, average pore size 120 nm; porosity 60%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0115] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 160 °C for 19 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0116] Film formation: 0.23 g of aluminum nitrate nonahydrate and 0.84 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 170 °C for 4 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0117] The performance of the Al-bttotb membrane obtained in Comparative Example 4 was tested using the same method as in Example 1.

[0118] Example 5

[0119] Carrier pretreatment: The sheet-like porous alumina carrier (3mm thick, 22mm in diameter, average pore size 130nm, porosity 50%) prepared by pressing and sintering was polished sequentially with 800# and 1200# sandpaper. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water, respectively, and dried in a muffle furnace at 500℃ for 10h to obtain the pretreated alumina carrier.

[0120] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 22 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 230 °C for 16 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0121] Film formation: 97 mg of aluminum nitrate nonahydrate and 631 mg of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 170 °C for 5 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0122] Al-bttotb powder crystals were also present in the liquid of the reactor during the above film formation process. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0123] The Al-bttotb membrane obtained in Example 5 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0124] Comparative Example 5

[0125] Carrier pretreatment: The sheet-like porous alumina carrier (3mm, diameter 22mm, average pore size 130nm; porosity 50%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10h to obtain the pretreated alumina carrier.

[0126] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 22 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The pretreated alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 230 °C for 16 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0127] Film formation: 97 mg aluminum nitrate nonahydrate and 631 mg 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then vertically placed into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 130 °C for 5 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0128] The Al-bttotb membrane obtained above was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0129] Example 6

[0130] Carrier pretreatment: The sheet-like porous alumina carrier (4 mm, diameter 19 mm, average pore size 90 nm; porosity 30%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0131] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 16 mL of LDM, and 10 mL of 99 wt% formic acid was added as a growth regulator. The mixture was then sonicated for 10 minutes to obtain the modified carrier mixture. The dried alumina carrier was then placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers and reacted in an oven at 250 °C for 24 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0132] Film formation: 31 mg of aluminum chloride hexahydrate and 505 mg of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 160 °C for 6 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0133] Al-bttotb powder crystals were also present in the liquid of the reactor during the above film formation process. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0134] The Al-bttotb membrane obtained in Example 6 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0135] Example 7

[0136] Carrier pretreatment: The sheet-like porous alumina carrier (thickness 4 mm, diameter 20 mm, average pore size 110 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0137] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, followed by sonication for 10 minutes to obtain a modified mixture of the carrier. Then, the dried alumina carrier was placed vertically in a polytetrafluoroethylene liner containing the modified mixture using tweezers, and reacted in an oven at 180 °C for 12 h. After the reaction was completed, the alumina carrier was removed and rinsed twice with methanol to remove uncoordinated excess ligands.

[0138] Film formation: 32 mg of aluminum nitrate nonahydrate and 420 mg of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 150 °C for 7 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0139] Al-bttotb powder crystals were also present in the liquid of the reactor during the above film formation process. After filtration, the most probable pore size under the DFT model was obtained using the BET micropore testing method.

[0140] The Al-bttotb membrane obtained in Example 7 was subjected to performance testing, and the specific testing method was the same as in Example 1.

[0141] Comparative Example 6

[0142] Carrier pretreatment: The sheet-like porous alumina carrier (thickness 4 mm, diameter 20 mm, average pore size 110 nm; porosity 20%) prepared by pressing and sintering method was polished with 800# and 1200# sandpaper in sequence. The resulting alumina carrier was cleaned with anhydrous ethanol and deionized water respectively, and dried in a muffle furnace at 500℃ for 10 h to obtain the pretreated alumina carrier.

[0143] Carrier modification: 0.8 g of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid was dissolved in 20 mL of LDM, followed by ultrasonic dissolution for 10 minutes to obtain a modified carrier mixture. Then, the pretreated alumina carrier was vertically placed in a polytetrafluoroethylene liner containing the modified solution using tweezers and kept at room temperature for 12 hours. After that, the alumina carrier was removed and rinsed twice with methanol to remove surface ligands.

[0144] Film formation: 32 mg of aluminum nitrate nonahydrate and 420 mg of 4,4',4”-(phenyl-1,3,5-trioxo)-benzoic acid were added to 30 mL of DMF and sonicated until completely dissolved. The two were then mixed and stirred for 30 minutes. Then, 10 mL of 99 wt% formic acid solution was slowly added while stirring. After complete mixing and thorough stirring, the MOF synthesis solution was obtained. The modified porous alumina support was then placed vertically into a reactor. The MOF synthesis solution was poured into a reactor lined with polytetrafluoroethylene. The reactor was then sealed and heated in an oven at 150 °C for 7 days. After the reaction was completed, the membrane was cooled to room temperature, removed, and gently washed in DMF. The membrane was then immersed in fresh anhydrous methanol for 12 h for activation. Finally, it was removed and dried at 50 °C for 12 h to obtain the Al-bttotb membrane.

[0145] The performance of the Al-bttotb membrane obtained in Example 6 was tested using the same method as in Example 1.

[0146] The results of single-component gas permeability (density), thermal stability and chemical stability tests, and pervaporation tests of the MOF membranes prepared in each specific embodiment and comparative example are shown in the table below.

[0147] Table 1

[0148]

[0149]

[0150] Note: The compactness effect data in this table is in H... 2 / As a comparison, the Knudsen diffusion selectivity of C3H8 was 4.69.

[0151] The stability and permeability of the membranes prepared in Comparative Examples 1 and 4-6 were not tested in the table above. This is because the density of the membrane material is a prerequisite for its separation effect on C6 alkane isomers (high density is required for separation). Furthermore, after sufficient density and separation selectivity are achieved, stability testing is conducted to further demonstrate its usability under more demanding conditions. The membranes prepared in the above comparative examples have very poor density; therefore, their stability and permeability were not further tested. The membranes prepared in Comparative Examples 2-3 underwent density and permeability testing. Due to their poor permeability, their stability was not further tested. The compactness of each MOF membrane is illustrated using H2 / C3H8 as an example. As shown in the table above, the Al-bttotb membrane provided by this invention is stable within the range of 80–125°C, exhibiting the highest H2 / C3H8 selectivity of 38.3. The total mass fraction of n-hexane and 3-methylpentane was increased from 67% on the feed side to 87% on the permeate side, while 2,2-dimethylbutane decreased from 33% to 13%. In contrast, the H2 / C3H8 selectivity obtained in the comparative example reached a maximum of 4.6. Therefore, the Al-bttotb membrane provided by this invention demonstrates superior compactness, stability, and permeability compared to the comparative example, exhibiting excellent separation performance for C6 alkane isomers. Furthermore, the MOF membranes prepared in Examples 2–7 were also tested according to the chemical stability test method described in Example 1. The results show that the MOF membranes prepared in each example all possess excellent chemical stability.

[0152] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.

Claims

1. A method for the preparation of MOF membranes for the efficient separation of C6 alkane isomers, characterized in that, The method comprises the following steps: carrier pretreatment: polishing, cleaning and drying the surface of the sheet-shaped porous alumina carrier to obtain a pretreated alumina carrier; carrier modification: dissolving 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid in a solvent to obtain a modification mixture; then vertically placing the pretreated alumina carrier in the modification mixture and heating at 180-250 ℃, and then taking out for rinsing and drying to obtain a modified alumina carrier; film formation: dissolving metal precursor salt, 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid and growth regulator in a solvent to obtain a MOF synthesis solution; then vertically placing the modified alumina carrier in the MOF synthesis solution and heating at 150-180 ℃ to obtain a MOF film. The MOF structure has a one-dimensional pore channel with a pore size of 5.4-6.0 Å.

2. The production method according to claim 1, wherein The MOF film is a one-dimensional pore channel structure Al-bttotb.

3. The production method according to claim 1, wherein In the carrier modification step, the heating time is 12-24 h.

4. The production method according to claim 1, wherein In the modification mixture, the molar ratio of the solvent to the 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid is 100:1-200:

1.

5. The production method according to claim 1, wherein In the MOF synthesis solution, the molar ratio of the 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid to the metal ions in the metal precursor salt is 1:1-10:1, the molar ratio of the solvent to the 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid is 200:1-600:1, and the molar ratio of the growth regulator to the 4,4',4''-(phenyl-1,3,5-trioxo)-benzoic acid is 50:1-380:

1.

6. The production method according to claim 1, wherein In the carrier modification step and film formation, the solvent is selected from a combination of one or more of methanol, ethanol, water and N,N-dimethylformamide; The growth regulator is selected from formic acid.

7. The production method according to claim 1, wherein In the carrier pretreatment step, the sheet-shaped porous alumina carrier has a thickness of 1-5 mm, a diameter of 18-25 mm, and an average pore size of 80-150 nm; the porosity is 20%-60%.

8. The production method according to claim 1, wherein In the film formation step, the metal precursor salt is selected from any one of aluminum nitrate nonahydrate, aluminum sulfate and aluminum chloride hexahydrate.

9. The production method according to claim 1, wherein It also comprises an activation step: soaking and drying the MOF film obtained in the film formation step in a solvent.

Citation Information

Patent Citations

  • Hybrid material containing metal organic framework material, and preparation method thereof

    CN109721737A

  • Aluminum-based metal-organic skeleton material and preparation method therefor, adsorption separation device, and method for separating hydrocarbon mixture

    WO2021196258A1