Fe / mn bimetallic nanocomposite, preparation method and application thereof

By preparing a core-shell structure of Fe/Mn bimetallic nanocomposite materials, the problems of low efficiency and poor stability in hydrogen peroxide synthesis were solved, realizing efficient in-situ synthesis and controllable decomposition of hydrogen peroxide, which significantly removes antibiotics from water and has good application prospects.

CN117654533BActive Publication Date: 2026-11-24FUJIAN NORMAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311422535.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-24
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Existing methods for synthesizing hydrogen peroxide suffer from high energy consumption, pollution byproducts, photocorrosion, and low yield. The efficiency and stability of in-situ synthesis of hydrogen peroxide using zero-valent iron and metallic Mn catalysts need to be improved.

Method used

Fe/Mn bimetallic nanocomposites were prepared by a one-step reduction method. In the core-shell structure, amorphous manganese oxide encapsulates zero-valent iron, forming a tightly contacted composite material. By utilizing its abundant structural defects and low valence state, efficient in-situ synthesis and controllable decomposition of hydrogen peroxide were achieved.

Benefits of technology

It achieves efficient production of hydrogen peroxide and controllable decomposition into hydroxyl radicals, significantly removing antibiotics from water. It has excellent separation performance and an environmentally friendly preparation process. The hydrogen peroxide content reaches 103.7 mg/L within 1 hour, and the enrofloxacin removal rate reaches 100%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117654533B_ABST
    Figure CN117654533B_ABST
Patent Text Reader

Abstract

This invention discloses an Fe / Mn bimetallic nanocomposite material, its preparation method, and its application, belonging to the field of catalytic material preparation technology. This invention prepares a core-shell structure rich in oxygen vacancies using a one-step sodium borohydride reduction method. This core-shell structure not only possesses numerous structural defects and exhibits excellent electron transfer capabilities and a high specific surface area, but also achieves effective close contact between iron and manganese. The shell structure composed of amorphous manganese oxide can synthesize hydrogen peroxide in situ, while the core structure composed of zero-valent iron can both synthesize hydrogen peroxide in situ and activate the synthesized hydrogen peroxide, producing a synergistic effect for efficient in-situ hydrogen peroxide production under oxygen-introduced conditions. The Fe / Mn bimetallic nanocomposite material of this invention shows significant removal effects on antibiotics in water and exhibits excellent separation performance. When the dosage is 4 g / L, the hydrogen peroxide content in the water reaches as high as 103.7 mg / L after 1 hour, and the removal rate of enrofloxacin at a concentration of 10 mg / L is 100% within 1 hour.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic material preparation technology, specifically relating to an Fe / Mn bimetallic nanocomposite material, its preparation method, and its application. Background Technology

[0002] Hydrogen peroxide (H2O2), as an environmentally friendly, pollution-free, and easily treated oxidant, has been widely used in chemical synthesis, disinfection, and environmental remediation. Furthermore, due to its high efficiency and ease of storage, it is a promising clean energy source. Currently, the main methods for synthesizing hydrogen peroxide include direct synthesis, electrochemical catalysis, and photochemical catalysis. Despite numerous efforts, these methods still suffer from some unavoidable problems. These include the high energy consumption and generation of polluting organic byproducts associated with direct synthesis; the high energy consumption and secondary reduction degradation of hydrogen peroxide into water in electrochemical catalysis; and the photochemical catalysis method, which is mainly plagued by photocorrosion and low yield.

[0003] Zero-valent metals and low-valence metals are often used for in-situ production of hydrogen peroxide. Zero-valent iron (Fe) stands out among many zero-valent metals due to its good safety and practicality. Fe can be used to activate oxygen, thereby generating hydrogen peroxide in situ. Mn and Fe are both transition metals in the periodic table, sharing some physicochemical properties with Fe, having abundant valence states, low toxicity, and excellent catalytic activity. Wang et al. used Fe-Mn catalysts to activate oxygen and remove norfloxacin from water; Li et al. prepared bimetallic catalysts using Mn doping to synergistically activate hydroxyl radicals and demonstrated the high catalytic performance of Mn-based catalysts. Furthermore, studies have shown that manganese compounds have excellent affinity for oxygen under normal conditions. The in-situ synthesis of H2O2 is affected by various factors. Adjusting the structure and properties of catalyst materials can alter the yield of H2O2. Moreover, zero-valent metal composite materials have the same ability to generate hydrogen peroxide in situ as zero-valent metals, and compared to single zero-valent metals, composite zero-valent metal materials have a larger specific surface area, which is beneficial for obtaining more active sites and improving the efficiency of in-situ hydrogen peroxide production. Therefore, improving the zero-valent iron process from the perspective of composite materials, enhancing the catalytic performance of zero-valent iron, and developing a method for in-situ efficient production of hydrogen peroxide using bimetallic nanocomposite materials composed of zero-valent or low-valent materials have significant research and practical value.

[0004] Patent CN114534683A discloses a core-shell magnetic nanomaterial, its preparation method, and its uses. In this invention, the nano-zero-valent iron coated in the material can remain stable and unoxidized for a long time. Furthermore, nano-zero-valent iron of different sizes, after being coated with iron-manganese oxide, can effectively remove heavy metal ions and organic pollutants from water. However, this material is synthesized using a two-step method, which is complex, and the manganese oxide coating the zero-valent iron only serves as a protective layer. Patent CN113908878A provides a preparation method and application of a bimetallic Prussian blue analog catalyst. This catalyst uses surfactants, potassium ferricyanide, and rare earth metal cerium salts as precursors. By controlling parameters such as time, pH, solvent, and temperature, a one-step crystallization growth method is used to grow a bimetallic Prussian blue analog structure rich in unsaturated active sites. However, this material can only effectively activate hydrogen peroxide and cannot achieve in-situ synthesis of hydrogen peroxide or controllable activation of hydrogen peroxide for the removal of antibiotics. Summary of the Invention

[0005] This invention discloses an Fe / Mn bimetallic nanocomposite material, its preparation method and application, wherein the bimetallic nanocomposite material is described.

[0006] The technical solution of the present invention is as follows:

[0007] One of the objectives of this invention is to provide a Fe / Mn bimetallic nanocomposite material, wherein the bimetallic nanocomposite material has a core-shell structure, wherein amorphous manganese oxide constitutes the shell structure and zero-valent iron constitutes the core structure, and amorphous manganese oxide grows in situ on the surface of the core structure to form a shell structure that tightly encapsulates the core structure.

[0008] The second objective of this invention is to provide a method for preparing Fe / Mn bimetallic nanocomposite materials.

[0009] Furthermore, this includes the following steps:

[0010] (1) Under normal temperature conditions, FeCl3·6H2O and MnSO4 are dissolved in organic solvents and mixed evenly.

[0011] (2) Dissolve sodium borohydride in ultrapure water and add it dropwise to the mixed solution prepared in step (1) by stirring at a constant speed until the two react completely.

[0012] (3) After the reaction is complete, the suspension is filtered and washed with ethanol several times before being placed in a vacuum drying oven to dry the bimetallic nanocomposite material.

[0013] Furthermore, in step (1), the molar ratio of iron and manganese in FeCl3·6H2O and MnSO4 is (0-3):(0-2), where the values ​​cannot both be 0.

[0014] Furthermore, in step (1), the organic solvent is a mixture of 10 mL of water and 40 mL of ethanol.

[0015] Furthermore, according to the chemical equation:

[0016] Fe 3+ +3BH4 - +3H₂O→Fe 0 +3B(OH)3+4.5H2

[0017] Mn 2+ +2BH4 - +H₂O→MnO x +2B(OH)3+2H2

[0018] In step (2), the minimum concentration of sodium borohydride is the minimum concentration required to completely reduce the amount of FeCl3·6H2O and MnSO4.

[0019] Furthermore, nitrogen gas is introduced for protection during the reduction process of sodium borohydride in step (1) and the filtration process of the suspension in step (3).

[0020] Furthermore, the filtration process in step (3) uses a circulating water vacuum pump.

[0021] Furthermore, in step (3), the drying temperature is 55-65℃ and the drying time is 12-24h.

[0022] The third objective of this invention is to provide an application of Fe / Mn bimetallic nanocomposite material in the in-situ synthesis of hydrogen peroxide.

[0023] Furthermore, the Fe / Mn bimetallic nanocomposite material can efficiently synthesize and collect hydrogen peroxide in situ under oxygen-introduced conditions, and controllably decompose the prepared hydrogen peroxide into hydroxyl radicals.

[0024] The fourth objective of this invention is to provide an application of Fe / Mn bimetallic nanocomposite material in the removal of antibiotics from water.

[0025] Furthermore, the Fe / Mn bimetallic nanocomposite material can remove enrofloxacin from water. When the dosage of the bimetallic nanocomposite material in the solution is 4 g / L, the removal rate of enrofloxacin at a concentration of 10 mg / L is 100% within 1 hour.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] 1. This invention prepares a Fe / Mn bimetallic nanocomposite material with a core-shell structure and rich in oxygen vacancies through a one-step reduction method using sodium borohydride. This core-shell structure not only has excellent electron transfer ability and high specific surface area, but also enables effective close contact between iron and manganese. The shell structure composed of amorphous manganese oxide can synthesize hydrogen peroxide in situ, while the core structure composed of zero-valent iron can not only synthesize hydrogen peroxide in situ, but also activate the synthesized hydrogen peroxide, thereby producing a synergistic effect. Under the condition of oxygen introduction, hydrogen peroxide is produced in situ with high efficiency.

[0028] 2. Unlike existing technologies that use manganese oxide to encapsulate zero-valent iron as a protective layer, this invention uses amorphous manganese oxide to encapsulate zero-valent iron. It utilizes the abundant structural defects, low valence state, and high reducing power of manganese oxide to enhance and improve its catalytic activity. Together with zero-valent iron, it participates in and optimizes the process of hydrogen peroxide synthesis. The encapsulated zero-valent iron can effectively prevent oxidation and controllably activate the in-situ synthesized hydrogen peroxide and decompose it into hydroxyl radicals.

[0029] 3. The Fe / Mn bimetallic nanocomposite material prepared by this invention can be applied to the field of water and soil environmental remediation. It has a significant effect on removing antibiotics from water and has excellent separation performance. It is easy to recover and the preparation method is simple and the synthesis process is environmentally friendly. When the dosage of this bimetallic nanocomposite material in the solution is 4 g / L, the hydrogen peroxide content in the water after 1 hour is as high as 103.7 mg / L. Moreover, the removal rate of enrofloxacin at a concentration of 10 mg / L can reach 100% within 1 hour. This invention has important practical significance and good application prospects for removing recalcitrant organic matter from water.

[0030] Figure Labels

[0031] Figure 1 The graphs show the synthesis of hydrogen peroxide from the Fe / Mn bimetallic nanocomposites prepared in Examples 1-4 and Comparative Examples 1-2 of this invention.

[0032] Figure 2 These are scanning electron microscope (SEM) images of the Fe / Mn bimetallic nanocomposites prepared in Example 1 and Comparative Examples 1-2 of this invention.

[0033] Figure 3 This is a transmission electron microscope image of the Fe / Mn bimetallic nanocomposite material prepared in Example 1 of the present invention;

[0034] Figure 4 The image shows the hysteresis loop of the Fe / Mn bimetallic nanocomposite material prepared in Example 1 of this invention.

[0035] Figure 5 The electron paramagnetic resonance image of the Fe / Mn bimetallic nanocomposite material prepared in Example 1 of this invention is shown.

[0036] Figure 6 The images show the effect of Fe / Mn bimetallic nanocomposite materials obtained in Example 1 and Comparative Examples 1-2 of this invention in removing enrofloxacin. Detailed Implementation

[0037] The present invention will be further described below with reference to the accompanying drawings and preferred embodiments. The embodiments given are only for illustrating the present invention and are not intended to limit the scope of the present invention.

[0038] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.

[0039] In the quantitative experiments in the following examples, three replicate experiments were set up, and the average value of the results was taken.

[0040] Unless otherwise specified, the experimental methods described in the following examples are conventional methods.

[0041] Example 1

[0042] This embodiment provides a Fe / Mn bimetallic nanocomposite material, the synthesis method of which includes the following steps:

[0043] S1. Under nitrogen protection, dissolve 6.4g FeCl3·6H2O and 1.8g MnSO4 in a mixed solvent of 10mL water and 40mL ethanol, respectively, and mix thoroughly.

[0044] S2. Dissolve 4g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared in S1 while stirring at a constant speed until the reaction is complete.

[0045] S3. After the reaction is complete, let it stand for 10 minutes. Then, under nitrogen protection, filter the resulting suspension using a circulating water vacuum pump. Rinse three times with ethanol and dry in a vacuum drying oven at 60°C for 18 hours to obtain the Fe:Mn = 2:1 bimetallic nanocomposite material. Scanning electron microscopy image as shown below. Figure 2 As shown in right 1.

[0046] The transmission electron microscope image of this bimetallic nanocomposite material is shown below. Figure 3 As shown in the figure, it can be clearly seen that the prepared novel Fe / Mn composite material has a core-shell chain structure, with Fe, Mn and O coexisting in the core, and the shell is an amorphous manganese oxide shell.

[0047] The hysteresis loop diagram of this bimetallic nanocomposite material is as follows: Figure 4 As shown in the figure, the catalyst is a typical soft magnetic material with excellent separation performance.

[0048] The electron paramagnetic resonance image of this bimetallic nanocomposite material is as follows: Figure 5 As shown, the composite doping of bimetals leads to lattice deformation and defects, resulting in oxygen vacancies in the prepared material.

[0049] Example 2

[0050] This embodiment provides a method for synthesizing Fe / Mn bimetallic nanocomposites, including the following steps:

[0051] S1. Under nitrogen protection, dissolve 3.2g FeCl3·6H2O and 3.6g MnSO4 in a mixed solvent of 10mL water and 40mL ethanol, respectively, and mix thoroughly.

[0052] S2. Dissolve 3.5g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared in S1 while stirring at a constant speed until the reaction is complete.

[0053] S3. After the reaction is complete, let it stand for 10 minutes. Under nitrogen protection, filter the obtained suspension using a circulating water vacuum pump. Rinse it three times with ethanol and dry it in a vacuum drying oven at 55°C for 24 hours to obtain the Fe:Mn=1:2 bimetallic nanocomposite material.

[0054] Example 3

[0055] This embodiment provides a method for synthesizing Fe / Mn bimetallic nanocomposites, including the following steps:

[0056] S1. Under nitrogen protection, dissolve 9.6g FeCl3·6H2O and 1.8g MnSO4 in a mixed solvent of 10mL water and 40mL ethanol, respectively, and mix thoroughly.

[0057] S2. Dissolve 5.5g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared in S1 while stirring at a constant speed until the reaction is complete.

[0058] S3. After the reaction is complete, let it stand for 10 minutes. Under nitrogen protection, filter the obtained suspension using a circulating water vacuum pump. Rinse it three times with ethanol and dry it in a vacuum drying oven at 65°C for 12 hours to obtain the Fe:Mn=3:1 bimetallic nanocomposite material.

[0059] Example 4

[0060] This embodiment provides a method for synthesizing Fe / Mn bimetallic nanocomposites, including the following steps:

[0061] S1. Under nitrogen protection, dissolve 9.6g FeCl3·6H2O and 5.4g MnSO4 in a mixed solvent of 10mL water and 40mL ethanol, respectively, and mix thoroughly.

[0062] S2. Dissolve 7.5g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared in S1 while stirring at a constant speed until the reaction is complete.

[0063] S3. After the reaction is complete, let it stand for 10 minutes. Under nitrogen protection, filter the obtained suspension using a circulating water vacuum pump. Rinse it three times with ethanol and dry it in a vacuum drying oven at 60°C for 18 hours to obtain Fe:Mn=1:1 bimetallic nanocomposite material.

[0064] Comparative Example 1

[0065] This comparative embodiment provides a method for synthesizing pure iron nanomaterials, including the following steps:

[0066] S1. Dissolve 9.6g FeCl3·6H2O in a mixed solvent of 10mL water and 40mL ethanol, and mix thoroughly.

[0067] S2. Dissolve 4g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared by S1, which is being stirred at a constant speed, until the reaction is complete.

[0068] S3. After the reaction is complete, let it stand for 10 minutes. Filter the resulting suspension using a circulating water vacuum pump, wash it three times with ethanol, and dry it in a vacuum drying oven to obtain the ZVI nanocomposite material. Figure 2 As shown in the second image from the left.

[0069] Comparative Example 2

[0070] This comparative embodiment provides a method for synthesizing pure manganese nanomaterials, including the following steps:

[0071] S1. Dissolve 5.4g MnSO4 in a mixed solvent of 10mL water and 40mL ethanol, and mix thoroughly.

[0072] S2. Dissolve 2.5g of sodium borohydride in 100ml of ultrapure water and add it dropwise to the mixed solution prepared by S1, which is being stirred at a constant speed, until the reaction is complete.

[0073] S3. After the reaction is complete, let it stand for 10 minutes. Filter the resulting suspension using a circulating water vacuum pump, wash it three times with ethanol, and dry it in a vacuum drying oven to obtain the ZVM nanocomposite material. Figure 2 As shown in the left image (1).

[0074] Performance testing

[0075] 1. Hydrogen peroxide production test

[0076] S1. Add 0.2g of the nanocomposite materials prepared in Examples 1-4 and Comparative Examples 1-2 to six reaction flasks containing 50mL of ultrapure water to prepare sample solutions. Place the reaction flasks on a magnetic stirrer at room temperature and introduce oxygen at a flow rate of 400mL / min to start the reaction.

[0077] S2. Prepare standard solutions of hydrogen peroxide at concentrations of 10 mg / L, 20 mg / L, 50 mg / L, 100 mg / L, 150 mg / L, and 200 mg / L, and determine their absorbance using potassium titanate ultraviolet spectrophotometry to obtain a standard curve of hydrogen peroxide absorbance.

[0078] S3. Take 2 mL of sample solution at 3 min, 5 min, 10 min, 15 min, 30 min, 40 min and 60 min. Add 1 mL of 3 mol / L H2SO4 and 1 mL of 0.05 mol / L potassium titanium oxalate solution to the sample solution, and then dilute to 10 mL with ultrapure water. Let it stand in the dark for 10 min, and measure the absorbance at 400 nm using a UV spectrophotometer. Obtain the hydrogen peroxide production by comparing with the hydrogen peroxide absorbance standard curve.

[0079] The yield curves of in-situ synthesis of hydrogen peroxide from Fe-Mn bimetallic nanocomposites prepared in Examples 1-4 and Comparative Examples 1-2 are shown below. Figure 1 As shown. By Figure 1 It can be seen that the solution with Fe:Mn = 2:1 (Example 1) had the highest hydrogen peroxide content at 60 min, reaching 103.7 mg / L; the solution in Example 2 had a hydrogen peroxide content of 10 mg / L at 60 min; the solution in Example 3 had a hydrogen peroxide content of 51.6 mg / L at 60 min; the solution in Example 4 had a hydrogen peroxide content of 68.9 mg / L at 60 min; the solution in Comparative Example 1 had a hydrogen peroxide content of 3.9 mg / L at 60 min; and the solution in Comparative Example 2 had a hydrogen peroxide content of 61.2 mg / L at 60 min. The results indicate that, compared to traditional pure iron or pure manganese nanomaterials, the Fe-Mn bimetallic nanocomposite material prepared in this invention exhibits superior in-situ hydrogen peroxide synthesis performance.

[0080] 2. Enrofloxacin removal test

[0081] S1. Prepare a 1 g / L enrofloxacin solution and dilute it to a concentration of 10 mg / L. Add 50 mL of the above diluent to each of the three reaction flasks and adjust the pH of the solution to 3. Add 0.2 g of the nanocomposite material prepared in Example 1 and Comparative Examples 1-2 to the three reaction flasks containing 10 mg / L enrofloxacin solution respectively. Place the reaction flasks on a magnetic stirrer at room temperature and introduce oxygen at a flow rate of 400 mL / min to start the reaction.

[0082] S2. Start timing simultaneously with the start of the reaction. At 3 min, 5 min, 10 min, 15 min, 30 min, 45 min, and 60 min, respectively, take 1 mL of liquid and filter it through a 0.22 μm pink filter. Detect the enrofloxacin content in the liquid using high-performance liquid chromatography (HPLC) and calculate the removal efficiency. Figure 6 .

[0083] The enrofloxacin removal effects of the Fe / Mn bimetallic catalysts prepared in Example 1, Comparative Example 1, and Comparative Example 2 are as follows: Figure 6 As shown, the results indicate that the bimetallic catalyst prepared in Example 1 achieved a 100% removal efficiency for enrofloxacin in 60 min; while the bimetallic catalyst prepared in Comparative Example 1 achieved a removal efficiency of 59.9% for enrofloxacin in 60 min, and the bimetallic catalyst prepared in Comparative Example 2 achieved a removal efficiency of 0% for enrofloxacin in 60 min. These results demonstrate that the bimetallic nanocomposite material of the present invention significantly improves the performance in removing enrofloxacin.

[0084] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. The application of a Fe / Mn bimetallic nanocomposite material in the in-situ synthesis of hydrogen peroxide, characterized in that, The bimetallic nanocomposite material has a core-shell structure, wherein amorphous manganese oxide forms the shell structure and zero-valent iron forms the core structure. Amorphous manganese oxide grows in situ on the surface of the core structure and forms a shell structure that tightly wraps the core structure. The preparation method of the Fe / Mn bimetallic nanocomposite material includes the following steps: (1) Under normal temperature conditions, FeCl3·6H2O and MnSO4 are dissolved in a mixed solvent of water and ethanol, respectively, and mixed evenly; (2) Dissolve sodium borohydride in ultrapure water and add it dropwise to the mixed solution prepared in step (1) by stirring at a constant speed until the two react completely. (3) After the reaction is complete, the suspension is filtered and washed with ethanol several times before being placed in a vacuum drying oven to dry the bimetallic nanocomposite material. Nitrogen gas is introduced for protection during the reduction process of sodium borohydride in step (2) and the filtration process of the suspension in step (3).

2. The application of the Fe / Mn bimetallic nanocomposite material as described in claim 1 in the in-situ synthesis of hydrogen peroxide, characterized in that, In step (1), the molar ratio of iron and manganese in FeCl3·6H2O and MnSO4 is (0-3):(0-2), where the value cannot be 0.

3. The application of the Fe / Mn bimetallic nanocomposite material as described in claim 1 in the in-situ synthesis of hydrogen peroxide, characterized in that, In step (1), the volume ratio of water to ethanol in the mixed solvent is 1:

4.

4. The application of the Fe / Mn bimetallic nanocomposite material as described in claim 1 in the in-situ synthesis of hydrogen peroxide, characterized in that, The drying temperature in step (3) is 55-65℃.

5. The application of the Fe / Mn bimetallic nanocomposite material as described in claim 1 in the in-situ synthesis of hydrogen peroxide, characterized in that, The drying time in step (3) is 12-24 hours.

Citation Information

Patent Citations

  • Preparation method and application of bimetallic Prussian blue analogue catalyst

    CN113908878A

  • Core-shell magnetic nano material as well as preparation method and application thereof

    CN114534683A