Metal-modified molecular sieve, process for the preparation thereof and process for the alkylation of long-chain olefins
By modifying the molecular sieve framework with a specific amount of metal, the problems of short catalyst lifetime and low product linearity were solved, achieving high-efficiency catalytic effect and low-cost production of long-chain olefin alkylation reaction.
Patent Information
- Application Number
- CN202211033764.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-08-26
AI Technical Summary
In existing technologies, molecular sieve-catalyzed alkylation of long-chain olefins has a short cycle life, low linearity of products, and a long preparation process with high cost.
Metal-modified molecular sieves are used, and a certain amount of metal is modified on the outside of the molecular sieve framework through two ion exchanges and two calcinations. The ratio of surface metal to bulk metal is controlled to not exceed 1.45, preferably 0.9-1.35. The metals are selected from alkaline earth metals and Group IIIB/IIIA metals. The preparation process is carried out under an alkaline atmosphere to ensure the stability of the molecular sieve structure.
It significantly improves the linearity of the product and the service life of the catalyst, extends the catalytic cycle, and reduces the preparation cost.
Smart Images

Figure CN117654587B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of molecular sieves, specifically to a metal-modified molecular sieve, its preparation method, and a method for alkylating long-chain olefins. Background Technology
[0002] Long-chain alkylbenzenes are important raw materials for the preparation of sodium alkylbenzene sulfonate, a synthetic detergent. Long-chain alkylbenzenes are mainly prepared by the alkylation reaction of long-chain olefins with monocyclic aromatic hydrocarbons. Current commercial processes primarily use HF or AlCl3 as catalysts, but these two catalytic systems pose significant safety and environmental risks and are gradually being phased out as safety and environmental requirements become increasingly stringent. Developing new, non-corrosive, and pollution-free solid acid alkylation methods as alternative technologies has become an inevitable trend in the production of long-chain alkylbenzenes.
[0003] Currently, industrial solid acid processes use a fluorine-containing SiO2-Al2O3 solid acid catalyst (CN1092755A) developed in cooperation between UOP (USA) and Petresa (Spain). However, because the catalyst itself contains fluorine, it is corrosive to equipment and still poses certain safety and environmental risks.
[0004] Domestic and international research has largely focused on zeolite molecular sieve catalyst systems. Due to the relatively large size of long-chain alkylbenzene molecules, channels with ten-membered rings or smaller cannot enter. Only molecular sieves such as MOR, Y, and Beta, which have channels with twelve-membered rings or larger, exhibit good catalytic performance in the alkylation reaction of benzene with long-chain olefins (Catal Surv Asia (2014) 18:1-12; Catal Today (2017) 298:109-116). Furthermore, because branched alkylbenzenes are not easily degraded, national standards impose strict requirements on the linearity of alkylbenzene products. The biggest problems with molecular sieve-catalyzed synthesis of long-chain alkylbenzenes are their short lifespan and low linearity.
[0005] For example, CN107867699A discloses a Y zeolite containing regular ultra-large micropores. By subjecting selected Y zeolite to template agent and acid-base treatment, a Y zeolite with regular ultra-large micropores of 1-2 nm is constructed. Due to the abundant acid centers and suitable reaction channels provided by the regular ultra-large micropores, higher conversion rate and selectivity are obtained.
[0006] CN110562995A discloses a method for synthesizing nano-Y zeolite and its application in the synthesis of straight-chain alkylbenzenes. Due to the small catalyst crystal size and low diffusion resistance, the activity and stability of long-chain olefin alkylation are improved.
[0007] CN102639471A discloses a method for producing linear alkylbenzenes, which uses a combination of two zeolites to limit skeletal isomerization and improve the linearity of the product.
[0008] However, in existing technologies, the alkylation cycle life of catalysts for long-chain olefins is still relatively short, the linearity of the product is low, and the preparation process is long and costly. Summary of the Invention
[0009] The purpose of this invention is to overcome the problems of short cycle life and low linearity of products in the alkylation of long-chain olefins by molecular sieve catalysis in the prior art. This invention provides a metal-modified molecular sieve, its preparation method and a method for alkylating long-chain olefins. The metal-modified molecular sieve contains a certain amount of extra-skeletal metal, which can effectively suppress skeletal isomerism of alkylbenzene products, improve the linearity of products, and at the same time significantly extend its catalytic alkylation cycle life.
[0010] To achieve the above objectives, the first aspect of the present invention provides a metal-modified molecular sieve, the metal-modified molecular sieve comprising a molecular sieve and a metal outside the molecular sieve framework; based on the total amount of the metal-modified molecular sieve, the content of the metal, in terms of elements, is 8-30 wt%.
[0011] In the metal-modified molecular sieve, the ratio of the mass fraction of the surface metal measured by XPS to the mass fraction of the bulk metal obtained by XRF test does not exceed 1.45, based on the mass fraction of elements.
[0012] A second aspect of this invention provides a method for preparing a metal-modified molecular sieve, comprising the following steps:
[0013] (1) The molecular sieve precursor is subjected to a first ion exchange with a first exchange solution containing a metal-soluble compound;
[0014] (2) The product of the first ion exchange is subjected to a first calcination to obtain the first exchange molecular sieve;
[0015] (3) The first exchange molecular sieve is subjected to a second ion exchange with a second exchange solution containing a metal-soluble compound;
[0016] (4) The product of the second ion exchange is subjected to a second calcination, and the second ion exchange and second calcination are optionally repeated to obtain the second exchange molecular sieve.
[0017] (5) The second exchange molecular sieve is subjected to high temperature treatment in an oxygen-containing atmosphere to obtain the metal-modified molecular sieve;
[0018] The first calcination and / or the second calcination are carried out under an alkaline atmosphere;
[0019] Based on the total amount of the metal-modified molecular sieve, the metal content is 8-30 wt% (elementally).
[0020] The third aspect of the present invention provides a metal-modified molecular sieve prepared by the above preparation method.
[0021] The fourth aspect of the present invention provides a method for alkylating long-chain olefins, the method comprising: contacting a long-chain olefin and an aromatic hydrocarbon with a catalyst under alkylation reaction conditions to carry out an alkylation reaction;
[0022] The catalyst is a metal-modified molecular sieve provided in the first or third aspect above.
[0023] The metal-modified molecular sieve provided by this invention, through modification with a certain amount of extra-skeletal metal, has a surface metal mass fraction measured by XPS and a bulk metal mass fraction measured by XRF that does not exceed 1.45. This effectively suppresses skeletal isomerism in alkylbenzene products, improves the linearity of the product, and significantly extends the catalytic alkylation cycle life.
[0024] The method for preparing metal-modified molecular sieves provided by this invention can achieve the modification of specific extra-framework metals through two cross-conversions and two calcinations, while ensuring the stability of the molecular sieve cell before and after the reaction and avoiding the destruction of the molecular sieve structure due to multiple calcinations.
[0025] The long-chain olefin alkylation method provided by this invention significantly improves the linearity of the product due to the shape selectivity of the reaction product after molecular sieve modification. The improved selectivity also significantly extends the catalytic alkylation cycle life of the metal-modified molecular sieve. Attached Figure Description
[0026] Figure 1 The XRD patterns of the metal-modified molecular sieve and HY molecular sieve prepared in Example 1 are shown in comparison.
[0027] Figure 2 The stability graph of the metal-modified molecular sieve prepared in Example 1 during the reaction of benzene with 1-dodecene to prepare linear alkylbenzene is obtained after 300 hours of continuous operation. Detailed Implementation
[0028] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0029] The first aspect of the present invention provides a metal-modified molecular sieve, the metal-modified molecular sieve comprising a molecular sieve and a metal outside the molecular sieve framework; based on the total amount of the metal-modified molecular sieve, the content of the metal is 8-30 wt% in terms of elements;
[0030] In the metal-modified molecular sieve, the ratio of the mass fraction of the surface metal measured by XPS to the mass fraction of the bulk metal obtained by XRF test does not exceed 1.45, based on the mass fraction of elements.
[0031] Through extensive research, the inventors of this invention discovered that molecular sieves containing a certain amount of extra-framework metal can effectively suppress skeletal isomerism in alkylbenzene products, improve the linearity of the product, and significantly extend the catalytic alkylation cycle life. In this invention, the "extra-framework metal" refers to metals existing in ionic form at the cation sites of the molecular sieve and / or loaded on the surface of the molecular sieve in oxide form. XRD testing reveals that the elution positions of the characteristic peaks of the metal-modified molecular sieve are the same as those of the unmodified molecular sieve, indicating no shift in the characteristic peaks. This confirms that the metals are located outside the molecular sieve framework.
[0032] The XRD test conditions include: the instrument used is an X-ray powder diffractometer from PANalytical, Netherlands; the test conditions include: tube voltage 40kV, tube current 40mA, Cu target Kα radiation, scanning speed 2° / min, and scanning range 2θ=5°-35°.
[0033] In this invention, the mass fraction of the surface metal refers to the mass fraction of the metal element obtained by XPS testing, and the mass fraction of the bulk metal refers to the mass fraction of the metal element obtained by XRF testing and calculation. It can be understood that XRF testing first obtains the mass fraction of the bulk metal as an oxide, and then the corresponding elemental mass fraction is calculated.
[0034] In this invention, an ESCALAB 250 X-ray photoelectron spectrometer (Thermo Fisher Scientific) was used for XPS testing. The test conditions included: monochromatic Al Kα X-rays, energy 1486.6 eV, power 150 W, and the charge shift was corrected using the C1s peak (284.8 eV) of contaminated carbon.
[0035] In this invention, an XRF test was performed using a Rigaku Electric Industrial Co., Ltd. 3271 X-ray fluorescence spectrometer. The test conditions included: the anode target material of the X-ray tube was a rhodium target; the laser voltage was 50 kV; and the laser current was 50 mA.
[0036] The inventors of this invention have made a creative discovery that the distribution of bulk metal and surface metal has a key influence on the catalytic performance of metal-modified molecular sieves in alkylation reactions. Under this distribution, byproduct generation and deactivation caused by olefin isomerization and polyalkylation reactions can be effectively suppressed, achieving shape-selective catalysis and thereby improving the linearity of the product and the cycle life of the molecular sieve.
[0037] According to the present invention, preferably, in the metal-modified molecular sieve, the ratio of the mass fraction of the surface metal measured by XPS to the mass fraction of the bulk metal obtained by XRF testing, based on the mass fraction of elements, does not exceed 1.35, preferably 0.9-1.35, for example, it can be 0.95, 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, or a value between two points. Under the above-mentioned preferred distribution, it is beneficial to improve the molecular sieve lifetime and the linearity of the product. If the ratio of the mass fraction of the surface metal to the mass fraction of the bulk metal is too high, it may lead to a shortened catalytic lifetime of the molecular sieve; if the ratio is too low, it may lead to a decrease in the linearity of the product.
[0038] In this invention, preferably, based on the total amount of the metal-modified molecular sieve, the metal content, in elemental terms, is 12-23 wt%. For example, the metal content, in elemental terms, can be 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, or any value between any two points. In the above preferred cases, it is beneficial to ensure that the metal distribution is in an optimal position, thereby achieving shape-selective catalysis, improving catalyst lifetime and product linearity.
[0039] In this invention, preferably, the atomic radius of the metal is 120-270 pm, more preferably 160-240 pm. Preferably, the metal is selected from at least one of alkaline earth metals, Group IIIB metals, and Group IIIA metals; preferably at least one of Mg, Ca, Sr, Ba, La, Ce, Pr, Rd, Sm, Eu, Yb, Sc, Y, Al, Ga, and In; more preferably at least one of La, Ce, Sr, and Y. Using the above-preferred metals facilitates matching with the molecular sieve channels, achieving optimal shape-selective catalysis, protecting the molecular sieve structure, and improving catalytic lifetime and product linearity.
[0040] In this invention, preferably, the metal-modified molecular sieve is a silica-alumina molecular sieve.
[0041] Preferably, the molar ratio of silicon oxide to aluminum oxide in the metal-modified molecular sieve is 1-100:1, and more preferably 3-20:1.
[0042] According to the present invention, preferably, the metal-modified molecular sieve is selected from at least one of X-type molecular sieves, Y-type molecular sieves, MCM-22 type molecular sieves, Beta type molecular sieves, and MOR type molecular sieves, and more preferably X-type molecular sieves and / or Y-type molecular sieves. Using the above-mentioned preferred types of molecular sieves is beneficial for further improving the catalytic activity of the molecular sieves.
[0043] A second aspect of this invention provides a method for preparing a metal-modified molecular sieve, comprising the following steps:
[0044] (1) The molecular sieve precursor is subjected to a first ion exchange with a first exchange solution containing a metal-soluble compound;
[0045] (2) The product of the first ion exchange is subjected to a first calcination to obtain the first exchange molecular sieve;
[0046] (3) The first exchange molecular sieve is subjected to a second ion exchange with a second exchange solution containing a metal-soluble compound;
[0047] (4) The product of the second ion exchange is subjected to a second calcination, and the second ion exchange and second calcination are optionally repeated to obtain a second exchange molecular sieve.
[0048] (5) The second exchange molecular sieve is subjected to high temperature treatment in an oxygen-containing atmosphere to obtain the metal-modified molecular sieve;
[0049] The first calcination and / or the second calcination are carried out under an alkaline atmosphere;
[0050] Based on the total amount of the metal-modified molecular sieve, the metal content is 8-30 wt% (elementally).
[0051] The method for preparing metal-modified molecular sieves provided by this invention can achieve the modification of specific extra-framework metals through at least two cross-conversions and two calcinations, while ensuring the stability of the cell size of the molecular sieve before and after the reaction, and avoiding the destruction of the molecular sieve structure due to multiple calcinations.
[0052] In this invention, the number of times the second ion exchange and the second calcination are repeated is not particularly limited and can be determined according to the effect of the ion exchange. The purpose is to ensure that the metal content in the molecular sieve meets the above-mentioned range requirements. For example, it can be repeated 1-3 times.
[0053] According to the present invention, preferably, the molecular sieve precursor is a silica-alumina molecular sieve, and the molar ratio of silica to alumina in the molecular sieve is preferably 1-100:1, more preferably 3-20:1.
[0054] In this invention, the molar ratio of silicon oxide to aluminum oxide in the molecular sieve remains essentially unchanged before and after metal modification, both satisfying the above-mentioned molar ratio range requirements.
[0055] According to the present invention, preferably, the molecular sieve precursor is selected from at least one of X-type molecular sieve, Y-type molecular sieve, MCM-22 type molecular sieve, Beta type molecular sieve and MOR type molecular sieve, and more preferably X-type molecular sieve and / or Y-type molecular sieve.
[0056] According to the present invention, preferably, the molecular sieve precursor is a hydrogen-form or sodium-form molecular sieve.
[0057] Preferably, the molecular sieve precursor is a sodium-type molecular sieve, and the first and / or second exchange liquids further include ammonium salts, for example, the first exchange liquid further includes ammonium salts. In this case, step (1) includes ion co-exchange of the sodium-type molecular sieve with a first exchange liquid containing a metal-soluble compound and an ammonium salt.
[0058] In this invention, the ammonium salt can be any conventional choice in the art. Preferably, the ammonium salt is selected from at least one of ammonium nitrate, ammonium chloride, and ammonium sulfate.
[0059] In this invention, preferably, the concentration of the ammonium salt is 50-200 g / L, more preferably 70-150 g / L.
[0060] According to the present invention, when the molecular sieve precursor is a sodium-type molecular sieve, preferably, the preparation method further includes ammonium exchange of the second exchange molecular sieve with a third exchange solution containing ammonium salt, followed by the high-temperature treatment.
[0061] In this invention, the ammonium exchange and drying can be carried out using conventional methods and conditions in the art. For example, the second exchange molecular sieve can be subjected to ammonium exchange, followed by filtration and drying, as one ammonium exchange process. The ammonium exchange process can optionally be repeated 1-3 times, so that the Na mass fraction in the molecular sieve is less than 0.2%.
[0062] In this invention, the concentration of ammonium salt in the third exchange liquid can be in the same range as that in the first or second exchange liquid, which will not be elaborated here.
[0063] In this invention, there is no particular limitation on the specific type of soluble compound of the metal, as long as a metal source can be provided, it can be selected according to actual needs. Preferably, the soluble compound of the metal is selected from at least one of the following: metal chloride, nitrate, phosphate, and sulfate.
[0064] According to the present invention, there is no particular limitation on the concentration of the metal-soluble compound in the first exchange liquid and / or the second exchange liquid, as long as the metal element content in the metal-modified molecular sieve meets the above-mentioned range requirements. Those skilled in the art can make conventional adjustments. Preferably, the concentration of the metal-soluble compound in the first exchange liquid and the second exchange liquid is independently 100-500 g / L, more preferably 130-400 g / L. Using the above-mentioned preferred embodiments, the preparation process can be shortened while meeting the above-mentioned content requirements.
[0065] Preferably, the first and second exchange solutions each independently include a solvent, and the solvent is preferably water.
[0066] In this invention, preferably, the atomic radius of the metal is 120-270 pm, more preferably 160-240 pm. Preferably, the metal is selected from at least one of alkaline earth metals, Group IIIB metals, and Group IIIA metals; preferably at least one of Mg, Ca, Sr, Ba, La, Ce, Pr, Rd, Sm, Eu, Yb, Sc, Y, Al, Ga, and In; more preferably at least one of La, Ce, Sr, and Y. Using the above-preferred metals facilitates matching with the molecular sieve channels, achieving optimal shape-selective catalysis, protecting the molecular sieve structure, improving catalyst lifetime, and increasing product linearity.
[0067] According to the present invention, in order to make the first ion exchange more complete, preferably, the mass ratio of the first exchange liquid to the molecular sieve precursor is 2-8:1, more preferably 3-6:1.
[0068] Preferably, the mass ratio of the second exchange liquid to the first exchange molecular sieve is 3-6:1, and more preferably 3-5:1.
[0069] In this invention, preferably, the conditions for the first ion exchange include: an exchange temperature of 50-90°C, more preferably 70-90°C; and an exchange time of 0.5-2 h, more preferably 0.8-1.5 h.
[0070] In this invention, the conditions for the second ion exchange can be the same as or different from those for the first ion exchange. Preferably, the conditions for the second ion exchange include: an exchange temperature of 50-120°C, more preferably 70-100°C; and an exchange time of 0.5-2 h, more preferably 0.8-1.5 h. Preferably, the exchange temperature of the second ion exchange is 0-15°C higher than that of the first exchange, more preferably 1-10°C. Using the above-mentioned preferred embodiments is beneficial for optimizing metal distribution and further improving the catalytic activity of the molecular sieve.
[0071] According to the present invention, preferably, based on the total amount of the metal-modified molecular sieve, the metal content, in terms of elemental composition, is 12-23 wt%. For example, the metal content, in terms of elemental composition, can be 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, or any value between any two points. Using the above-mentioned preferred metal content helps ensure that the metal distribution is in an optimal position, thereby achieving shape-selective catalysis and improving the molecular sieve lifetime and product linearity.
[0072] In this invention, to further control the distribution of the metal, the first calcination and / or the second calcination are carried out under an alkaline atmosphere. Preferably, both the first and second calcinations are carried out under an alkaline atmosphere. Adopting the above-mentioned preferred embodiments helps to protect the molecular sieve structure and further improve the catalytic lifetime of the metal-modified molecular sieve.
[0073] According to the present invention, preferably, the alkaline atmosphere is provided by an aqueous solution of an alkaline compound. It is understood that the aqueous solution of the alkaline compound rapidly vaporizes at the calcination temperature, thereby providing an alkaline atmosphere for the calcination process.
[0074] In this invention, the range of alkaline compounds is relatively wide. Preferably, the alkaline compound is selected from at least one of ammonia, ammonium carbonate, and urea, with ammonia being the most preferred.
[0075] In this invention, preferably, the concentration of the alkaline compound in the aqueous solution is 0.01-2 mol / L, more preferably 0.01-0.5 mol / L, and even more preferably 0.05-0.3 mol / L. Under the above preferred conditions, it is beneficial to the stability of the molecular sieve structure and to extend the cycle life of molecular sieve catalytic alkylation.
[0076] According to the present invention, preferably, the alkaline atmosphere introduction rate is 0.01-0.5 mL / min relative to 50 g of molecular sieve precursor, more preferably 0.05-0.2 mL / min. It is understood that the alkaline atmosphere introduction rate can be increased proportionally as the amount of molecular sieve precursor processed increases.
[0077] Preferably, the conditions for the first calcination include: a calcination temperature of 400-600℃, a calcination time of 0.5-3h, and a pressure of 0.01-0.1MPa, wherein the pressure is gauge pressure.
[0078] Preferably, the conditions for the second calcination include: a calcination temperature of 400-600℃, a calcination time of 0.5-3h, and a pressure of 0.01-0.1MPa, wherein the pressure is gauge pressure.
[0079] In this invention, the first and second roasting do not refer to the order of operations, but are only used to distinguish the roasting conditions in different steps. The conditions for the first and second roasting can be the same or different, as long as the above-mentioned requirements are met.
[0080] In this invention, before the first or second calcination, the product of the first or second ion exchange is subjected to solid-liquid separation and drying. The solid-liquid separation and drying can be performed using conventional operations in the art, and will not be described in detail here.
[0081] According to the present invention, preferably, the oxygen-containing atmosphere is air or a mixture of oxygen and an inert gas; the inert gas is preferably nitrogen.
[0082] In this invention, preferably, the oxygen content in the oxygen-containing atmosphere is 16-30 vol%, more preferably 18-25 vol%.
[0083] Preferably, the high-temperature treatment temperature is 50-100°C higher than the second calcination temperature.
[0084] According to the present invention, preferably, the conditions for the high-temperature treatment include: a temperature of 500-700℃, more preferably 550-650℃, and a treatment time of 2-12h, more preferably 4-8h.
[0085] The third aspect of the present invention provides a metal-modified molecular sieve prepared by the above preparation method.
[0086] The fourth aspect of the present invention provides a method for alkylating long-chain olefins, the method comprising: contacting a long-chain olefin and an aromatic hydrocarbon with a catalyst under alkylation reaction conditions to carry out an alkylation reaction;
[0087] The catalyst is the metal-modified molecular sieve described in the first or third aspect.
[0088] In this invention, the shape selectivity of the reaction products after molecular sieve modification significantly improves the linearity of the products, and the improved selectivity also significantly extends the catalytic alkylation cycle life of the metal-modified molecular sieve.
[0089] In this invention, there are no special requirements regarding the source of the long-chain olefins. For example, long-chain olefins obtained through dehydrogenation, cracking, or oligomerization of small molecule olefins can be used in this invention. Preferably, the long-chain olefins are long-chain olefins with double bonds at both the terminal and internal positions, and / or long-chain α-olefins with double bonds at the terminal position.
[0090] Preferably, the long-chain olefin is a C8-C28 long-chain olefin, more preferably a C8-C15 long-chain olefin, and even more preferably a C10-C14 long-chain olefin.
[0091] According to the present invention, preferably, the aromatic hydrocarbon is selected from at least one of benzene, toluene and ethylbenzene, and preferably benzene.
[0092] In this invention, the alkylation reaction conditions can be carried out under conditions conventional in the art, preferably ensuring that the alkylation reaction is carried out in a liquid phase and that the pressure is always sufficient to ensure that the reaction proceeds in a single liquid phase. In this invention, the term "single liquid phase" refers to the fact that all reactants are in a liquid phase, and the reaction conditions ensure that the reactants do not vaporize during the reaction.
[0093] In this invention, preferably, the conditions for the alkylation reaction include: a reaction temperature of 50-250°C, more preferably 70-200°C; a reaction pressure of 0.1-7 MPa, more preferably 2-4 MPa; a benzene-olefin molar ratio of 3-70:1, more preferably 4-60:1; and a space velocity of 0.1-5 h⁻¹ for the long-chain olefin. -1 Preferably 0.3-3h -1 Using the above-mentioned preferred reaction conditions helps to reduce alkyl isomerization and minimize the polyalkylation of benzene (or the aromatic moiety of other aryl compounds), while maximizing the consumption of olefins to maximize the product yield.
[0094] Preferably, the alkylation reaction is carried out in a slurry bed reactor.
[0095] The present invention will be described in detail below through embodiments.
[0096] In the following embodiments, unless otherwise specified, all raw materials used are commercially available.
[0097] In the following embodiments, the mass fraction of the bulk metal was determined by XRF testing. The mass fraction of the surface metal was determined by XPS testing.
[0098] In this invention, an ESCALAB 250 X-ray photoelectron spectrometer (Thermo Fisher Scientific) was used for XPS testing. The test conditions included: monochromatic Al Kα X-rays, energy 1486.6 eV, power 150 W, and the charge shift was corrected using the C1s peak (284.8 eV) of contaminated carbon.
[0099] In this invention, an XRF test was performed using a Rigaku Electric Industrial Co., Ltd. 3271 X-ray fluorescence spectrometer. The test conditions included: the anode target material of the X-ray tube was a rhodium target; the laser voltage was 50 kV; and the laser current was 50 mA.
[0100] The XRD test conditions include: the instrument used is an X-ray powder diffractometer from PANalytical, Netherlands; the test conditions include: tube voltage 40kV, tube current 40mA, Cu target Kα radiation, scanning speed 2° / min, and scanning range 2θ=5°-35°.
[0101] The molecular sieves used in the following examples were all purchased from Sinopec Catalyst Co., Ltd.
[0102] Example 1
[0103] (1) Take 50g of HY molecular sieve (molar ratio of silicon oxide / alumina is 6, w(Na2O)=0.0628%), and perform the first ion exchange on the HY molecular sieve with lanthanum nitrate solution. The concentration of lanthanum nitrate is 300g / L, the exchange temperature is 80℃, the exchange time is 1h, and the mass ratio of lanthanum nitrate solution to HY molecular sieve is 3:1. After the exchange, the molecular sieve is filtered and dried, and then calcined at 550℃ for 1h under a pressure of 0.02MPa. During the calcination process, 0.1M ammonia water is introduced at 0.1mL / min. After calcination, the first exchange molecular sieve is obtained, and the mass fraction of lanthanum metal is calculated to be 10.65% by XRF detection.
[0104] (2) The first exchange molecular sieve is subjected to a second ion exchange and a second calcination to obtain a second exchange molecular sieve under the same conditions as in step 1. The mass fraction of lanthanum metal in the second exchange molecular sieve is calculated to be 17.33% by XRF detection.
[0105] (3) The second exchange molecular sieve is calcined in an air atmosphere in a muffle furnace at 600°C for 4 hours to obtain the finished molecular sieve, which is numbered Y1.
[0106] Through XRD testing, such as Figure 1 As shown, the characteristic peaks at 11.9° and 12.4° belong to the metal ions at the cation sites, and the characteristic peak at 29.0° belongs to the metal oxides on the surface of the molecular sieve. At the same time, by comparing with the diffraction peaks of HY molecular sieve, it can be seen that the peak positions of the characteristic peaks of the metal-modified molecular sieve are the same as those of the diffraction peaks of HY molecular sieve, that is, there is no shift. This proves that the metals are all located outside the molecular sieve framework.
[0107] The physicochemical properties of the molecular sieve Y1 obtained by testing are shown in Table 1.
[0108] Example 2
[0109] The method was followed as in Example 1, except that the HY-type molecular sieve in (1) was replaced with an equal mass of Hβ-type molecular sieve (the molar ratio of silicon oxide to aluminum oxide was 19, and w(Na2O) = 0.0171%). The resulting metal-modified molecular sieve was designated Y2.
[0110] The physicochemical properties of the molecular sieve Y2 obtained from the test are shown in Table 1.
[0111] Example 3
[0112] The method described in Example 1 was followed, except that the lanthanum nitrate solution was replaced with a cerium nitrate solution. The resulting metal-modified molecular sieve was designated Y3.
[0113] The physicochemical properties of the molecular sieve Y3 obtained from the test are shown in Table 1.
[0114] Example 4
[0115] The method described in Example 1 was followed, except that the lanthanum nitrate solution was replaced with a strontium nitrate solution. The resulting metal-modified molecular sieve was designated Y4.
[0116] The physicochemical properties of the molecular sieve Y4 obtained by testing are shown in Table 1.
[0117] Example 5
[0118] The method was followed as in Example 1, except that the mass ratio of lanthanum nitrate solution to HY molecular sieve was 2.5:1 in both the first and second ion exchanges. The resulting metal-modified molecular sieve was designated Y5.
[0119] The physicochemical properties of the molecular sieve Y5 obtained from the test are shown in Table 1.
[0120] Example 6
[0121] The method was followed as in Example 1, except that the mass ratio of lanthanum nitrate solution to HY molecular sieve was 3.8:1 in both the first and second ion exchanges. The resulting metal-modified molecular sieve was designated Y6.
[0122] The physicochemical properties of the molecular sieve Y6 obtained by testing are shown in Table 1.
[0123] Example 7
[0124] The method described in Example 1 was followed, except that the ammonia flow rate was changed to 0.03 mL / min. The resulting metal-modified molecular sieve was designated Y7.
[0125] The physicochemical properties of the molecular sieve Y7 obtained from the test are shown in Table 1.
[0126] Example 8
[0127] (1) Take 50g of NaY molecular sieve (the molar ratio of silicon dioxide / alumina is 5, w(Na2O) = 12.8%), and use a mixed solution of ammonium chloride and lanthanum nitrate to carry out the first ion exchange of NaY molecular sieve. The concentration of ammonium chloride is 120g / L (calculated separately), the concentration of lanthanum nitrate is 300g / L (calculated separately), the exchange temperature is 80℃, the exchange time is 1h, and the mass ratio of the mixed solution to the molecular sieve is 3:1. After the exchange, the molecular sieve is filtered and dried, and then calcined at 550℃ for 1h under a pressure of 0.02MPa. During the calcination process, 0.1M ammonia water is introduced at 0.1mL / min. The first exchange molecular sieve is obtained after calcination.
[0128] (2) The first exchange molecular sieve is subjected to a second ion exchange and a second calcination to obtain a second exchange molecular sieve, under the same conditions as in step 1.
[0129] (3) The second exchange molecular sieve was exchanged with ammonium chloride solution. The concentration of ammonium chloride was 120 g / L, the exchange temperature was 80 °C, the exchange time was 1 h, and the mass ratio of ammonium chloride solution to molecular sieve was 3:1. After the exchange, the molecular sieve was filtered and dried, and then exchanged with ammonium chloride solution again under the same conditions as above. This was repeated twice to make the Na mass fraction in the molecular sieve less than 0.2%. The second exchange molecular sieve was then calcined in a muffle furnace at 600 °C for 4 h in an air atmosphere.
[0130] This is the finished molecular sieve, designated Y8. The physicochemical properties of the tested molecular sieve Y8 are shown in Table 1.
[0131] Example 9
[0132] The method was followed as in Example 1, except that the concentration of the lanthanum nitrate solution was 400 g / L. The resulting metal-modified molecular sieve was designated Y9.
[0133] The physicochemical properties of the molecular sieve Y9 obtained from the test are shown in Table 1 (continued).
[0134] Example 10
[0135] The method was followed as in Example 1, except that the concentration of the lanthanum nitrate solution was 200 g / L. The resulting metal-modified molecular sieve was designated Y10.
[0136] The physicochemical properties of the molecular sieve Y10 obtained from the test are shown in Table 1 (continued).
[0137] Example 11
[0138] The method was followed as in Example 1, except that the HY-type molecular sieve in (1) was replaced with an equal mass of HX-type molecular sieve (the molar ratio of silicon oxide to aluminum oxide was 2, and w(Na2O) = 0.0156%). The resulting metal-modified molecular sieve was designated Y11.
[0139] The physicochemical properties of the molecular sieve Y11 obtained from the test are shown in Table 1 (continued).
[0140] Example 12
[0141] (1) Take 50g of HY molecular sieve (the molar ratio of silicon oxide / alumina is 6, w(Na2O)=0.0628%), and use lanthanum nitrate solution to carry out the first ion exchange of HY molecular sieve. The concentration of lanthanum nitrate is 300g / L, the exchange temperature is 80℃, the exchange time is 1h, and the mass ratio of lanthanum nitrate solution to HY molecular sieve is 3:1. After the exchange, the molecular sieve is filtered and dried, and then calcined at 550℃ for 1h under a pressure of 0.02MPa. During the calcination process, 0.1M ammonia water is introduced at 0.1mL / min to obtain the first exchange molecular sieve.
[0142] (2) The first exchange molecular sieve is subjected to a second ion exchange, which is different from the first ion exchange in that the second ion exchange temperature is 90℃; after calcination, the second exchange molecular sieve is obtained.
[0143] (3) The second exchange molecular sieve is calcined in an air atmosphere in a muffle furnace at 600°C for 4 hours to obtain the finished molecular sieve, which is numbered Y12.
[0144] The physicochemical properties of the molecular sieve Y12 obtained from the test are shown in Table 1 (continued).
[0145] Comparative Example 1
[0146] The untreated HY molecular sieve from Example 1 was used, designated DY1. The physicochemical properties of the obtained molecular sieve DY1 are shown in Table 1 (continued).
[0147] Comparative Example 2
[0148] (1) Take 50g of HY molecular sieve (molar ratio of silicon oxide / alumina is 6, w(Na2O) = 0.0628%), and perform the first ion exchange on the HY molecular sieve with lanthanum nitrate solution. The concentration of lanthanum nitrate is 150g / L, the exchange temperature is 80℃, the exchange time is 1h, and the mass ratio of solution to molecular sieve is 3:1. After the exchange, the molecular sieve is filtered and dried, and then calcined at 550℃ for 1h under a pressure of 0.02MPa. At the same time, 0.1M ammonia water is introduced at 0.1mL / min during the calcination process. After calcination, the first exchange molecular sieve is obtained, and the mass fraction of lanthanum metal is calculated to be 5.83% by XRF detection.
[0149] (2) The first exchange molecular sieve is subjected to a second ion exchange and a second calcination to obtain a second exchange molecular sieve under the same conditions as in step 1. The mass fraction of lanthanum metal in the second exchange molecular sieve is calculated to be 6.97% by XRF detection.
[0150] (3) The second exchange molecular sieve is calcined in an air atmosphere in a muffle furnace at 600°C for 4 hours to obtain the finished molecular sieve, which is numbered DY2.
[0151] The physicochemical properties of the molecular sieve DY2 obtained from the test are shown in Table 1 (continued).
[0152] Comparative Example 3
[0153] (1) Take 50g of HY molecular sieve (molar ratio of silicon oxide / alumina is 6, w(Na2O) = 0.0628%), and perform the first ion exchange on the HY molecular sieve with lanthanum nitrate solution at a concentration of 900g / L, an exchange temperature of 80℃, an exchange time of 1h, and a solution-to-molecular sieve mass ratio of 3:1. After the exchange, the molecular sieve is evaporated to remove water and dried, and then calcined at 550℃ for 1h under a pressure of 0.02MPa. At the same time, 0.1M ammonia water is introduced at 0.1mL / min during the calcination process. After calcination, the mass fraction of lanthanum metal in the molecular sieve is calculated to be 19.06% by XRF detection.
[0154] (2) The first exchange molecular sieve is subjected to a second ion exchange and a second calcination to obtain a second exchange molecular sieve. The method is the same as in step 1. The mass fraction of lanthanum metal in the second exchange molecular sieve is calculated to be 31.80% by XRF detection.
[0155] (3) The second exchange molecular sieve is calcined in an air atmosphere in a muffle furnace at 600°C for 4 hours to obtain the finished molecular sieve, which is numbered DY3.
[0156] The physicochemical properties of the molecular sieve DY3 obtained by testing are shown in Table 1 (continued).
[0157] Comparative Example 4
[0158] The method in Example 1 was followed, except that an equal amount of water was introduced to replace ammonia in both the first and second calcination processes. The resulting molecular sieve was denoted as DY4. The physicochemical properties of the obtained molecular sieve DY4 are shown in Table 1 (continued).
[0159] Table 1
[0160]
[0161] Continued from Table 1
[0162]
[0163]
[0164] Test Example 1
[0165] The molecular sieve sample Y1 from Example 1 was subjected to an alkylation reaction of benzene with 1-dodecene under reaction conditions of 120°C and 2.5 MPa, with an olefin feed space velocity of 0.354 h⁻¹.-1 The molar ratio of styrene to phenylene was 60. The conversion and product selectivity results under these reaction conditions are shown in Table 2.
[0166] The stability of the molecular sieve from Example 1 was evaluated, and the results are shown in [Figure 1]. Figure 2 ,from Figure 2 It can be seen that the molecular sieve prepared in Example 1 has stable catalytic performance in the alkylation reaction of 1-dodecene and benzene. In the evaluation of 300h, the selectivity of monoalkylbenzene is close to 100%, and the linearity of alkylbenzene is also above 94%.
[0167] Conversion rate of 1-dodecene (%) = (Amount of 1-dodecene before reaction - Amount of 1-dodecene after reaction) / Amount of 1-dodecene before reaction × 100%.
[0168] Monoalkylbenzene selectivity (%) = Amount of monoalkylbenzene after reaction / Amount of all reaction products × 100%;
[0169] Straight-chain degree (%) = Amount of straight-chain alkylbenzene after reaction / Amount of monoalkylbenzene after reaction × 100%.
[0170] Test Example 2-12
[0171] Following the method of Test Example 1, Y1 was replaced with the molecular sieves from Examples 2-12, respectively. The alkylation reaction results are shown in Table 2 and Table 2 (continued).
[0172] Comparative test cases 1-4
[0173] Following the method in Test Example 1, Y1 was replaced with the molecular sieves used in Comparative Examples 1-4, respectively. The alkylation reaction results are shown in Table 2 (continued).
[0174] Table 2
[0175]
[0176]
[0177] Continued from Table 2
[0178]
[0179] As can be seen from the results in Table 2 and Table 2 (continued), the metal-modified molecular sieve prepared in the embodiments of the present invention exhibits high activity, stability, and selectivity in catalyzing the alkylation reaction of 1-dodecene with benzene, with a monoalkylbenzene selectivity of over 98% and a linear chain degree of over 94% for the alkylbenzene.
[0180] A comparison of Example 1 and Comparative Examples 1-3 shows that the absence of metal modification, excessively high or low metal content are detrimental to improving catalyst lifetime and product linearity. In particular, when the metal content exceeds 30 wt%, the olefin conversion rate decreases significantly, and the selectivity for monoalkylbenzenes is poor. Examples 1 and Comparative Example 4 show that when neither the first nor second calcination uses an alkaline atmosphere, the mass fraction of surface metal is higher, leading to reduced catalyst activity, decreased linearity of alkylbenzenes, and a rapid decline in catalytic effect and catalyst lifetime as the reaction proceeds.
[0181] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A metal-modified molecular sieve, characterized in that, The metal-modified molecular sieve comprises a molecular sieve and a metal outside the molecular sieve framework; based on the total amount of the metal-modified molecular sieve, the metal content, expressed as an element, is 12-23 wt%. The metal-modified molecular sieve is an X-type molecular sieve and / or a Y-type molecular sieve, and the molar ratio of silica to alumina in the metal-modified molecular sieve is 1-20:1; In the metal-modified molecular sieve, the ratio of the mass fraction of the surface metal measured by XPS to the mass fraction of the bulk metal obtained by XRF testing is 0.9-1.35, based on the mass fraction of elements.
2. The metal-modified molecular sieve according to claim 1, wherein, The atomic radius of the metal is 120-270 pm.
3. The metal-modified molecular sieve according to claim 2, wherein, The atomic radius of the metal is 160-240 pm.
4. The metal-modified molecular sieve according to claim 1, wherein, The metal is selected from at least one of alkaline earth metals, Group IIIB metals, and Group IIIA metals.
5. The metal-modified molecular sieve according to claim 4, wherein, The metal is selected from at least one of La, Ce, Sr and Y.
6. The method for preparing the metal-modified molecular sieve according to any one of claims 1-5, characterized in that, Includes the following steps: (1) The molecular sieve precursor is subjected to a first ion exchange with a first exchange solution containing a metal-soluble compound; (2) The product of the first ion exchange is subjected to a first calcination to obtain the first exchange molecular sieve; (3) The first exchange molecular sieve is subjected to a second ion exchange with a second exchange solution containing a metal-soluble compound; (4) The product of the second ion exchange is subjected to a second calcination, and the second ion exchange and second calcination are optionally repeated to obtain the second exchange molecular sieve; (5) The second exchange molecular sieve is subjected to high temperature treatment in an oxygen-containing atmosphere to obtain the metal-modified molecular sieve; The first calcination and / or the second calcination are carried out under an alkaline atmosphere.
7. The preparation method according to claim 6, wherein, The molecular sieve precursor is a hydrogen-type or sodium-type molecular sieve.
8. The preparation method according to claim 6, wherein, The molecular sieve precursor is a sodium-type molecular sieve, and the first and / or second exchange liquids also contain ammonium salts.
9. The preparation method according to claim 8, wherein, The ammonium salt is selected from at least one of ammonium nitrate, ammonium chloride, and ammonium sulfate.
10. The preparation method according to claim 9, wherein, In the first and / or second exchange solutions, the concentration of ammonium salts is independently 50-200 g / L.
11. The preparation method according to claim 6, wherein, The soluble compound of the metal is selected from at least one of the metal chloride, nitrate, phosphate and sulfate.
12. The preparation method according to claim 6, wherein, In the first and / or second exchange solutions, the concentration of the soluble compound of the metal is independently 100-500 g / L.
13. The preparation method according to claim 6, wherein, The first and second exchange liquids each independently include a solvent.
14. The preparation method according to claim 13, wherein, The solvent is water.
15. The preparation method according to claim 6, wherein, The mass ratio of the first exchange liquid to the molecular sieve precursor is 2-8:
1.
16. The preparation method according to claim 6, wherein, The mass ratio of the second exchange liquid to the first exchange molecular sieve is 3-6:
1.
17. The preparation method according to claim 6, wherein, The conditions for the first ion exchange include: an exchange temperature of 50-90℃ and an exchange time of 0.5-2h.
18. The preparation method according to claim 17, wherein, The conditions for the first ion exchange include: an exchange temperature of 70-90℃ and an exchange time of 0.5-1.5h.
19. The preparation method according to claim 6, wherein, The exchange temperature of the second ion exchange is 0-15℃ higher than that of the first ion exchange.
20. The preparation method according to claim 19, wherein, The exchange temperature of the second ion exchange is 1-10℃ higher than that of the first ion exchange.
21. The preparation method according to claim 6, wherein, The alkaline atmosphere is provided by an aqueous solution of an alkaline compound.
22. The preparation method according to claim 21, wherein, The alkaline compound is selected from at least one of ammonia, ammonium carbonate, and urea.
23. The preparation method according to claim 21, wherein, The concentration of the alkaline compound in the aqueous solution is 0.01-2 mol / L.
24. The preparation method according to claim 6, wherein, The alkaline atmosphere was introduced at a rate of 0.01-0.5 mL / min relative to 50 g of molecular sieve precursor.
25. The preparation method according to claim 6, wherein, The conditions for the first calcination include: a calcination temperature of 400-600℃, a calcination time of 0.5-3h, and a pressure of 0.01-0.1MPa, wherein the pressure is gauge pressure.
26. The preparation method according to claim 6, wherein, The conditions for the second calcination include: a calcination temperature of 400-600℃, a calcination time of 0.5-3h, and a pressure of 0.01-0.1MPa, wherein the pressure is gauge pressure.
27. The preparation method according to claim 6, wherein, The oxygen-containing atmosphere is air or a mixture of oxygen and an inert gas.
28. The preparation method according to claim 27, wherein, The oxygen content in the oxygen-containing atmosphere is 16-30 vol.
29. The preparation method according to claim 28, wherein, The oxygen content in the oxygen-containing atmosphere is 18-25 vol.
30. The preparation method according to claim 6, wherein, The high-temperature treatment temperature is 50-100°C higher than the second roasting temperature.
31. The preparation method according to claim 6, wherein, The conditions for the high-temperature treatment include: a temperature of 500-700℃ and a treatment time of 2-12 hours.
32. The preparation method according to claim 31, wherein, The conditions for the high-temperature treatment include: a temperature of 550-650℃ and a treatment time of 4-8 hours.
33. A method for alkylating long-chain olefins, the method comprising: Under alkylation reaction conditions, long-chain olefins and aromatics are contacted with a catalyst to carry out alkylation reaction; The catalyst is characterized in that it is a metal-modified molecular sieve as described in any one of claims 1-5.
34. The method according to claim 33, wherein, The long-chain olefin is a long-chain olefin with double bonds at both the terminal and internal positions, and / or a long-chain α-olefin with double bonds at the terminal position.
35. The method according to claim 34, wherein, The long-chain olefins are C8-C28 long-chain olefins.
36. The method according to claim 35, wherein, The long-chain olefin is a C8-C15 long-chain olefin.
37. The method according to claim 36, wherein, The long-chain olefins are C10-C14 long-chain olefins.
38. The method according to claim 33, wherein, The aromatic hydrocarbon is at least one of benzene, toluene, and ethylbenzene.
39. The method according to claim 38, wherein, The aromatic hydrocarbon is benzene.
40. The method according to claim 33, wherein, The alkylation reaction conditions include: a reaction temperature of 50-250℃; a reaction pressure of 0.1-7 MPa; a molar ratio of aromatics to long-chain olefins of 3-70:1; and a mass hourly space velocity (HHSV) of 0.1-5 h⁻¹ for the long-chain olefins. -1 .
41. The method according to claim 40, wherein, The conditions for the alkylation reaction include: a reaction temperature of 70-200℃; a reaction pressure of 2-4 MPa; a molar ratio of aromatics to long-chain olefins of 4-60:1; and a mass hourly space velocity (HHSV) of 0.3-3 h⁻¹ for the long-chain olefins. -1 .
Citation Information
Patent Citations
Alkylation process using catalysts with low olefin skeletal isomerization activity
CN102639471A
Y-zeolite containing structured ultra-large micropores, and preparation method and application thereof
CN107867699A
Benzene alkylation process using a fluorided silica-alumina and a linear C6 to C20 monoolefin
CN1092755A
Synthesis method of nano Y zeolite, synthesized nano Y zeolite and application
CN110562995A
Rare earth Y-type molecular sieve and preparation method thereof
CN103508467A