A method for manufacturing an AuSn sealing local gold plating pre-melting cover plate
By forming a raised arc-shaped connection between the AuSn alloy solder ring and the cover plate through vacuum heating and formic acid treatment, the problems of weak welding and voids are solved, and efficient and low-cost hermetic sealing cover plate manufacturing is achieved.
Patent Information
- Application Number
- CN202311732121.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-14
AI Technical Summary
In existing technologies, the welding of hermetic sealing covers is not firm and is prone to falling off. Furthermore, traditional methods require special equipment, which increases costs, and the welding quality is not high, resulting in voids and reliability issues.
AuSn alloy solder rings are welded to the cover plate semi-finished product in a vacuum furnace. Through vacuum heating and formic acid treatment, a raised arc-shaped connection is formed to avoid oxidation and achieve a firm bond between the AuSn alloy and the cover plate body.
It reduced production costs, improved weld strength and sealing reliability, reduced porosity, and enhanced packaging strength and efficiency.
Smart Images

Figure CN117655445B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing an airtight sealing cover, specifically disclosing a method for manufacturing an AuSn fusion-sealed, partially gold-plated pre-melted cover. Background Technology
[0002] In the field of electronic packaging, hermetic packaging covers are widely used, especially in high-reliability packaging. This is because chips must be isolated from the outside environment to prevent corrosion of the chip circuitry by impurities in the air, which could lead to a decline in electrical performance. Therefore, the packaging must have excellent sealing performance, and the quality of the packaging technology directly affects the performance of the chip itself. Current packaging methods typically involve first using pulse spot welding to fix a gold-plated Kovar alloy sheet to an AuSn pre-formed solder pad. Then, the cover is placed on the sealing area of the ceramic housing, and reflow soldering melts the AuSn alloy pre-formed solder pad, assembling it with the lower housing to achieve a seal.
[0003] The method of using pulse spot welding to fix gold-plated Kovar alloy sheets to AuSn alloy preformed sheets has problems such as weak brazing connections and easy detachment. Moreover, this method requires special equipment, which increases costs, is not conducive to improving production efficiency, and may also damage the gold-plated Kovar alloy sheets or AuSn alloy preformed sheets.
[0004] Because the tungsten metal layer on the ceramic tube substrate shrinks during solidification, the metallized zone of the weld ring is concave in the middle and convex at both ends. Traditional fusion seal plates use flat solder, resulting in a gap between the solder ring and the welding surface of the tungsten metallized layer on the ceramic tube. If the solder flow is insufficient during welding, pores in the weld cannot escape, easily forming voids in the weld area.
[0005] In the utility model patent with publication number CN202172064U, a weld resistance layer is placed between the pre-formed weld sheet and the sealing cover plate, followed by reflow soldering to melt and fix the pre-formed weld sheet onto the surface of the sealing cover plate. However, the use of reflow soldering easily leads to oxidation of the weld sheet after melting, and the shape cannot be guaranteed. During the subsequent alloy sealing process, the gases emitted from its interior cannot escape, resulting in large-area holes between the cover plate and the welding ring after sealing, leading to decreased welding quality and reduced reliability. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for manufacturing an AuSn fusion-sealed partial gold-plated pre-melted cover plate that has a strong bond between the solder and the cover plate body, facilitates the discharge of pores in the weld during alloy fusion sealing, and is easy to implement.
[0007] According to the technical solution provided by the present invention, the method for manufacturing the AuSn fusion-sealed partial gold-plated pre-melted cover plate includes the following steps: S1. Take the cover plate semi-finished product and AuSn alloy solder ring. The cover plate semi-finished product includes a cover plate body, a side Au layer located on the side of the cover plate body, a front Au ring located on the upper surface of the cover plate body, a front Ni layer located inside the front Au ring on the upper surface of the cover plate body, a back Au ring located on the lower surface of the cover plate body, and a back Ni layer located inside the back Au ring on the lower surface of the cover plate body. The front Au ring and the AuSn alloy solder ring are dimensionally matched and ready for use. S2. First, stack the AuSn alloy solder rings on the front Au ring of the cover plate semi-finished product, then place it in the vacuum furnace. Next, evacuate the vacuum furnace, controlling the vacuum level to 10Pa - 1.0 × 10⁻⁶ Pa. -3 Pa; S3. The vacuum furnace is heated to 280-360℃ and held for 5-300 seconds. After the AuSn alloy solder ring melts, the upper surface of the molten metal forms a raised arc shape, so that the AuSn alloy solder ring is welded to the front Au ring. During the heating process, when the temperature exceeds 180℃, formic acid is introduced into the vacuum furnace to remove the oxide layer on the tin-rich surface, thereby further preventing solder oxidation. S4. After the heat preservation is completed, stop heating and allow the vacuum furnace to cool naturally to below 50°C. Then, open the vacuum furnace and remove the finished cover plate. The finished cover plate includes the cover plate body, the side Au layer located on the side of the cover plate body, the front Au ring located on the upper surface of the cover plate body, the AuSn alloy ring located on the upper surface of the front Au ring, the front Ni layer located on the upper surface of the cover plate body inside the front Au ring, the back Au ring located on the lower surface of the cover plate body, and the back Ni layer located on the lower surface of the cover plate body inside the back Au ring.
[0008] Preferably, the AuSn alloy solder ring contains 76-82 wt% Au and 18-24 wt% Sn.
[0009] Preferably, the cover plate body is made of Kovar alloy.
[0010] The manufacturing method of the present invention has the following advantages: 1) The sealing surface (i.e. the upper surface) of the cover plate body does not need to be plated with gold on the entire surface, which greatly reduces production costs; 2) AuSn alloy solder rings do not oxidize after melting and their shape is controllable, making them particularly suitable for shape control of small-sized pre-melted cover plates; 3) No flux cleaning is required if no flux is used; 4) The AuSn alloy solder is firmly bonded to the cover plate body; 5) After the AuSn alloy solder ring melts, it forms a raised arc shape, which helps to remove pores in the weld during alloy sealing, reduces porosity, and improves the strength and reliability of the sealing device. 6) Easy to implement, highly efficient, requires no additional equipment, and saves costs. Attached Figure Description
[0011] Figure 1 This is a structural diagram of the semi-finished cover plate.
[0012] Figure 2 This is a schematic diagram of the AuSn alloy solder ring.
[0013] Figure 3 This is a structural diagram of the finished cover plate. Detailed Implementation
[0014] The present invention will be further described below with reference to specific embodiments.
[0015] Example 1 A method for manufacturing an AuSn fusion-sealed partial gold-plated pre-melted cover plate, the method comprising the following steps: S1. Take the semi-finished cover plate 1 (e.g.) Figure 1 (as shown) and AuSn alloy solder ring 1 (as shown) Figure 2 As shown), the cover plate semi-finished product 1 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body 1.1, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1. The cover plate body 1.1 is made of Kovar alloy. In the AuSn alloy solder ring 2, the Au content is 76wt% and the Sn content is 24wt%. The front Au ring 1.3 and the AuSn alloy solder ring 2 are dimensionally matched and are ready for use. S2. First, place the AuSn alloy solder ring 2 on the front Au ring 1.3 of the cover plate semi-finished product 1 and put it into the vacuum furnace. Then, evacuate the vacuum furnace and control the vacuum degree of the vacuum furnace at 10Pa. S3. The vacuum furnace is heated to 280°C and held for 300 seconds. After the AuSn alloy solder ring 2 melts, the upper surface of the molten metal forms a raised arc shape, so that the AuSn alloy solder ring 2 is welded to the front Au ring 1.3. During the heating process, when the temperature exceeds 180°C, formic acid is introduced into the vacuum furnace to remove the oxide layer on the tin-rich surface, thereby further preventing solder oxidation. S4. After the heat preservation is completed, stop heating and allow the vacuum furnace to cool naturally to 45℃. Then, open the vacuum furnace and remove the cover plate of product 3 (e.g., ...). Figure 3As shown), the finished cover plate 3 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, an AuSn alloy ring 2.1 located on the upper surface of the front Au ring 1.3, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body 1.1, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1.
[0016] Example 2 A method for manufacturing an AuSn fusion-sealed partial gold-plated pre-melted cover plate, the method comprising the following steps: S1. Take the semi-finished cover plate 1 (e.g.) Figure 1 (as shown) and AuSn alloy solder ring 2 (as shown) Figure 2 As shown), the cover plate semi-finished product 1 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body 1.1, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1. The cover plate body 1.1 is made of Kovar alloy. In the AuSn alloy solder ring 2, the Au content is 80wt% and the Sn content is 20wt%. The front Au ring 1.3 and the AuSn alloy solder ring 2 are dimensionally matched and are ready for use. S2. First, place the AuSn alloy solder ring 2 on the front Au ring 1.3 of the cover plate semi-finished product 1 and put it into the vacuum furnace. Then, evacuate the vacuum furnace and control the vacuum degree of the vacuum furnace at 0.1 Pa. S3. The vacuum furnace is heated to 320℃ and held for 100 seconds. After the AuSn alloy solder ring 2 melts, the upper surface of the molten metal forms a raised arc shape, so that the AuSn alloy solder ring 2 is welded to the front Au ring 1.3. During the heating process, when the temperature exceeds 180℃, formic acid is introduced into the vacuum furnace to remove the oxide layer on the tin-rich surface, thereby further preventing solder oxidation. S4. After the heat preservation is completed, stop heating and allow the vacuum furnace to cool naturally to below 30°C. Then, open the vacuum furnace and remove the cover plate. (e.g., finished product 3) Figure 3As shown), the finished cover plate 3 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, an AuSn alloy ring 2.1 located on the upper surface of the front Au ring 1.3, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1.
[0017] Example 3 A method for manufacturing an AuSn fusion-sealed partial gold-plated pre-melted cover plate, the method comprising the following steps: S1. Take the semi-finished cover plate 1 (e.g.) Figure 1 (as shown) and AuSn alloy solder ring 2 (as shown) Figure 2 As shown), the cover plate semi-finished product 1 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body 1.1, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1. The cover plate body 1 is made of Kovar alloy. In the AuSn alloy solder ring 2, the Au content is 82wt% and the Sn content is 18wt%. The front Au ring 1.3 and the AuSn alloy solder ring 2 are dimensionally matched and are ready for use. S2. First, stack the AuSn alloy solder ring 2 on the front Au ring 1.3 of the cover plate semi-finished product 1, then place it in the vacuum furnace, and then evacuate the vacuum furnace to control the vacuum degree of the vacuum furnace at 1.0×10. -3 Pa; S3. The vacuum furnace is heated to 360°C and held for 5 seconds. After the AuSn alloy solder ring 2 melts, the upper surface of the molten metal forms a raised arc shape, so that the AuSn alloy solder ring 2 is welded to the front Au ring 1.3. During the heating process, when the temperature exceeds 180°C, formic acid is introduced into the vacuum furnace to remove the oxide layer on the tin-rich surface, thereby further preventing the solder from oxidizing. S4. After the heat preservation is completed, stop heating and allow the vacuum furnace to cool naturally to below 20°C. Then, open the vacuum furnace and remove the cover plate. (e.g., finished product 3) Figure 3As shown), the finished cover plate 3 includes a cover plate body 1.1, a side Au layer 1.2 located on the side of the cover plate body 1.1, a front Au ring 1.3 located on the upper surface of the cover plate body 1.1, an AuSn alloy ring 2.1 located on the upper surface of the front Au ring 1.3, a front Ni layer 1.4 located inside the front Au ring 1.3 on the upper surface of the cover plate body 1.1, a back Au ring 1.5 located on the lower surface of the cover plate body 1.1, and a back Ni layer 1.6 located inside the back Au ring 1.5 on the lower surface of the cover plate body 1.1.
[0018] This invention pre-melts the AuSn alloy solder ring 2 on the front Au ring 1.3 under a vacuum atmosphere to form a convex shape, which makes the AuSn alloy solder ring 2 and the front Au ring 1.3 firmly bonded and highly reliable. The AuSn alloy solder ring 2 does not oxidize after melting and its shape is controllable, making it particularly suitable for shape control of small-sized pre-melted cover plates.
[0019] The sealing surface of the cover plate semi-finished product 1 used in this invention does not require full-surface gold plating, which greatly reduces production costs. The pre-melting process does not use flux and does not require flux cleaning. Furthermore, the manufacturing method of this invention is easy to implement, highly efficient, and requires no additional equipment.
[0020] After the AuSn alloy solder ring 2 melts, it forms an upward convex arc shape. During alloy sealing, it helps to remove pores in the weld, reduces porosity, and improves the strength and reliability of the seal.
[0021] Finally, it should be noted that the above description is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for manufacturing an AuSn fusion-sealed, partially gold-plated pre-melted cover plate, characterized in that: The method includes the following steps: S1. Take the cover plate semi-finished product (1) and the AuSn alloy solder ring (2). The cover plate semi-finished product (1) includes the cover plate body (1.1), the side Au layer (1.2) located on the side of the cover plate body (1.1), the front Au ring (1.3) located on the upper surface of the cover plate body (1.1), the front Ni layer (1.4) located inside the front Au ring (1.3) on the upper surface of the cover plate body (1.1), the back Au ring (1.5) located on the lower surface of the cover plate body (1.1), and the back Ni layer (1.6) located inside the back Au ring (1.5) on the lower surface of the cover plate body (1.1). The front Au ring (1.3) and the AuSn alloy solder ring (2) are sized to match and are ready for use. S2. First, place the AuSn alloy solder ring (2) on the front Au ring (1.3) of the cover plate semi-finished product (1) and then put it into the vacuum furnace. Then, evacuate the vacuum furnace and control the vacuum degree of the vacuum furnace at 10Pa-1.0×10 -3 Pa; S3. The vacuum furnace is heated to 280-360℃ and held for 5-300 seconds. After the AuSn alloy solder ring (2) melts, the upper surface of the molten metal forms a raised arc shape, so that the AuSn alloy solder ring (2) is welded to the front Au ring (1.3). During the heating process, when the temperature exceeds 180℃, formic acid is introduced into the vacuum furnace to remove the oxide layer on the tin-rich surface, thereby further preventing the solder from oxidizing. S4. After the heat preservation is completed, stop heating and allow the vacuum furnace to cool naturally to below 50°C. Then open the vacuum furnace and take out the finished cover plate (3). The finished cover plate (3) includes the cover plate body (1.1), the side Au layer (1.2) located on the side of the cover plate body (1.1), the front Au ring (1.3) located on the upper surface of the cover plate body (1.1), the AuSn alloy ring (2.1) located on the upper surface of the front Au ring (1.3), the front Ni layer (1.4) located on the upper surface of the cover plate body (1.1) inside the front Au ring (1.3), the back Au ring (1.5) located on the lower surface of the cover plate body (1.1), and the back Ni layer (1.6) located on the lower surface of the cover plate body (1.1) inside the back Au ring (1.5). In the AuSn alloy solder ring (2), the content of Au is 76-82wt% and the content of Sn is 18-24wt%.
2. The method for manufacturing the AuSn fusion-sealed partial gold-plated pre-melted cover plate as described in claim 1, characterized in that: The material of the cover plate body (1.1) is Kovar alloy.
Citation Information
Patent Citations
Air tightness packaging cover plate precoated with solder layer
CN202172064U
Preparation method of cover plate pre-coated with solder
CN116810161A
Airtight packaging alloy solder cover plate and preparation method thereof
CN117059578A
Stave-machine
US31934A