Process for the preparation of linear alkylbenzenes

By preparing modified molecular sieve catalysts and controlling the distribution of rare earth elements in β-cage and supercage structures, the problems of low linearity and high isomerization in the production of linear alkylbenzenes were solved, thereby extending the catalyst lifetime and improving the linearity of the product.

CN117658756BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211035151.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2026-11-20
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

Existing technologies for the production of straight-chain alkylbenzenes suffer from problems such as low linearity and high isomerization of the target product, as well as short lifespan of molecular sieve catalysts.

Method used

Modified molecular sieves were used as solid acid catalysts. By controlling the distribution of rare earth elements in the β-cage and supercage structures, modified molecular sieves with specific R and K values ​​were prepared to inhibit the skeletal isomerization of straight-chain olefins and improve alkylation activity.

Benefits of technology

It effectively improves the linearity of the target product and the lifetime of the molecular sieve catalyst, thereby enhancing the selectivity of the alkylation reaction and the stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117658756B_ABST
    Figure CN117658756B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of alkylation reaction, and discloses a preparation method of linear alkylbenzene.The method comprises the following steps: under alkylation reaction conditions, linear olefin and aromatic hydrocarbon are subjected to contact reaction in the presence of a solid acid catalyst; wherein the solid acid catalyst comprises modified molecular sieve and a binder, the modified molecular sieve comprises molecular sieve and rare earth elements, the modified molecular sieve has beta cage and supercage structure, the R value of the modified molecular sieve is 10-35%, and the K value of the modified molecular sieve is 1-20; wherein the R value represents the mass fraction of rare earth elements in the modified molecular sieve in terms of oxides, and the K value represents the ratio of the content of rare earth elements in the beta cage and the supercage of the modified molecular sieve.The method can effectively inhibit the skeletal isomerization of linear olefin, improve the catalytic life of the catalyst and the linear degree of the target product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of alkylation reactions, and more specifically to a method for preparing linear alkylbenzenes. Background Technology

[0002] Linear alkylbenzenes are obtained by the alkylation reaction of linear olefins and benzene. Traditional linear alkylbenzene production processes mostly use liquid catalysts, such as HF and AlCl3. Existing traditional processes also suffer from various drawbacks, including environmental pollution, severe equipment corrosion, difficulty in separating the product from the alkylene, and high investment costs. Currently, the development of traditional acid-catalyzed processes is somewhat constrained; therefore, the development of novel, green, and environmentally friendly solid acid catalyst processes is urgently needed.

[0003] UOP and a Spanish oil company jointly developed the Detal solid acid process, which overcomes some of the shortcomings of the HF and AlCl3 processes. However, because the Detal process uses an amorphous silica-alumina catalyst containing F, the process requires frequent regeneration, F is lost during operation, the alkylation and catalyst regeneration processes are discontinuous, and the operating cost is high, which limits the promotion and development of the Detal solid acid process (Modern Chemical Industry, 2016, 45(2):373-375).

[0004] Existing research on molecular sieves for the catalytic synthesis of linear alkylbenzenes mainly focuses on Y, β and mordenite. The main problem is that the molecular sieves generally have short catalytic lifetimes and low linearity of the products (Bull. Korean Chem. Soc., 2001, 22(9): 1056-1058).

[0005] Patent application CN101861290A discloses a layered zeolite catalyst for improving linearity in detergent alkylation, wherein the catalyst comprises a layered composition comprising an inner core and an outer layer bonded to the inner core, and the catalyst is capable of improving the performance of the target product to a certain extent.

[0006] Patent application CN102655932A discloses a rare earth modified molecular sieve catalyst, which is synthesized by exchanging rare earth elements. Summary of the Invention

[0007] The purpose of this invention is to overcome the problems of low linearity and high isomerization of the target product in the preparation of linear alkylbenzenes in the prior art, and to provide a method for preparing linear alkylbenzenes that can effectively inhibit the skeletal isomerization of linear olefins and improve the linearity of the target product.

[0008] To achieve the above objectives, the present invention provides a method for preparing linear alkylbenzenes, the method comprising: reacting linear olefins and aromatics in the presence of a solid acid catalyst under alkylation reaction conditions;

[0009] The solid acid catalyst comprises a modified molecular sieve and a binder. The modified molecular sieve includes a molecular sieve and rare earth elements. The modified molecular sieve has β-cage and supercage structures. The R value of the modified molecular sieve is 10-35%, and the K value is 1-20. The R value represents the mass fraction of rare earth elements in the modified molecular sieve as oxides, and the K value represents the ratio of the rare earth element content in the β-cage to that in the supercage of the modified molecular sieve.

[0010] The inventors of this invention discovered in their research that isomerization of straight-chain olefins is the main reason for the low linearity of alkylation products and the short catalytic lifetime of molecular sieves. The method provided by this invention uses a modified molecular sieve with suitable rare earth loading and loading positions as a solid acid catalyst with active components, which effectively inhibits the skeletal isomerization of straight-chain olefins as a whole, while maintaining strong alkylation activity, so as to improve the catalytic lifetime of molecular sieves and improve the linearity of the target product. Attached Figure Description

[0011] Figure 1 This is a graph showing the trend of olefin conversion rate in Example 1 of the present invention;

[0012] Figure 2 This is a graph showing the trend of linearity of the target product in Embodiment 1 of the present invention. Detailed Implementation

[0013] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0014] This invention provides a method for preparing linear alkylbenzenes, wherein the method comprises: reacting linear olefins and aromatics in the presence of a solid acid catalyst under alkylation reaction conditions;

[0015] The solid acid catalyst comprises a modified molecular sieve and a binder. The modified molecular sieve includes a molecular sieve and rare earth elements. The modified molecular sieve has β-cage and supercage structures. The R value of the modified molecular sieve is 10-35%, and the K value is 1-20. The R value represents the mass fraction of rare earth elements in the modified molecular sieve as oxides, and the K value represents the ratio of the rare earth element content in the β-cage to that in the supercage of the modified molecular sieve.

[0016] In a preferred embodiment, the R value of the modified molecular sieve is 16-28%, for example, it can be 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, and any value between any two groups.

[0017] In the preparation method provided by the present invention, modified molecular sieves are selected as the active component of solid acid catalysts. By controlling the total amount of rare earth elements in the modified molecular sieves, the molecular sieve channels can be modified, the molecular sieve structure can be strengthened, the generation of reaction by-products can be suppressed, and the selectivity of the main product can be improved.

[0018] In a preferred embodiment, the K value of the modified molecular sieve is 2-8, for example, it can be 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, or any value between two groups. In the preparation method provided by this invention, by controlling the distribution of rare earth elements in the β-cages and supercages of the modified molecular sieve, the pores of the molecular sieve can be modified and the linearity of the target product can be improved.

[0019] This invention provides a preparation method in which rare earth elements are selected to modify molecular sieves, thereby loading a high content of rare earth elements into the molecular sieves. At the same time, the distribution of rare earth elements in the β cage and supercage is controlled to form a specific distribution. This allows the modified molecular sieve to effectively inhibit the skeletal isomerization of linear olefins in the preparation of linear alkylbenzenes, while also exhibiting strong alkylation activity. This aims to improve the catalytic lifetime of the modified molecular sieves and increase the linearity of the target product.

[0020] In this invention, the "R value" is measured by XRF. The instrument used is a Rigaku Electric Industrial Co., Ltd. 3271 X-ray fluorescence spectrometer. The test conditions are: the anode target material of the X-ray tube is a rhodium target; the laser voltage is 50kV; and the laser current is 50mA.

[0021] In this invention, the "K value" is obtained by XRD. The instrument used is Netherland, PANalytical Corporation. The test conditions are: tube voltage 40kV, tube current 40mA, Cu target Kα radiation, scanning speed 2° / min, scanning range 2θ=5°-35°. The "K value" is calculated by the ratio of the area of ​​the characteristic peak at 11.9° to the area of ​​the characteristic peak at 12.4° in the XRD spectrum.

[0022] In a preferred embodiment, the B value of the modified molecular sieve is 1.1-1.5, preferably 1.2-1.4. The B value represents the mass fraction ratio of rare earth elements (calculated as oxides) in the surface phase and bulk phase of the modified molecular sieve. The B value can be, for example, 1, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, or any value between any two groups. The advantage of this preferred embodiment is that the molecular sieve surface modification suppresses side reactions.

[0023] In this invention, "the rare earth element content (mass fraction) in the bulk phase of the modified molecular sieve, calculated as oxides" refers to the mass fraction of rare earth elements in the modified molecular sieve, calculated as oxides, as mentioned above, i.e., the R value. In this invention, "the rare earth element content (mass fraction) in the bulk phase of the modified molecular sieve, calculated as oxides" is measured by XRF. The specific instrument used is a Rigaku Electric Industrial Co., Ltd. 3271 X-ray fluorescence spectrometer; the test conditions are: the anode target material of the X-ray tube is a rhodium target; the laser voltage is 50kV; and the laser current is 50mA.

[0024] In this invention, the "rare earth element content (mass fraction) in the modified molecular sieve surface phase, calculated as oxides" is obtained through XPS measurement. Specifically, the XPS measurement conditions are as follows: Instrument used: ESCALAB250 X-ray photoelectron spectrometer, manufactured by Thermo Fisher Scientific; Test conditions: monochromatic Al Kα X-rays, energy 1486.6 eV, power 150 W, with charge shift corrected using the C1s peak (284.8 eV) of contaminating carbon. It is understood that in this invention, the XPS measurement first obtains the mole fraction of surface rare earth elements as elements, and then the mass fraction of surface rare earth elements as oxides is calculated.

[0025] In this invention, there is no particular limitation on the type of modified molecular sieve; any molecular sieve conventionally defined in the art is applicable to this invention. Preferably, the modified molecular sieve is a silica-alumina molecular sieve.

[0026] In a preferred embodiment, the silicon-to-aluminum molar ratio of the modified molecular sieve is 1-50, more preferably 1.5-9. In this invention, it is understood that the silicon-to-aluminum molar ratio refers to the molar ratio of silicon atoms to aluminum atoms.

[0027] In this invention, rare earth elements are loaded at specific positions of the molecular sieve, and the pores and surface of the modified molecular sieve are modified to improve the shape selectivity of the modified molecular sieve for alkylation reactions.

[0028] In this invention, a wide range of rare earth elements are selected. Preferably, the rare earth elements are selected from Sc, Y, and non-radioactive lanthanides.

[0029] In a preferred embodiment, the rare earth element is selected from at least one of Sc, Y, La, Ce, Pr, Nd, Sm, and Yb, and more preferably La and / or Ce. Using the above-mentioned preferred rare earth elements facilitates matching between the rare earth elements and the molecular sieve channels, achieving optimal shape-selective catalysis, protecting the molecular sieve structure, and improving catalyst lifetime and the linearity of the target product.

[0030] In a preferred embodiment, the method for preparing the modified molecular sieve includes:

[0031] (1) Place the molecular sieve in a rare earth element ion exchange solution and perform the first ion exchange calcination. Treat the calcination product with acid in an acid solution. Repeat the above steps at least once to obtain the first ion exchange product.

[0032] (2) The first ion exchange product is placed in the rare earth element ion exchange solution for a second ion exchange, and the above steps are repeated at least once to obtain the second ion exchange product.

[0033] (3) The second ion exchange product is placed in a rare earth element ion exchange solution for rare earth oxide precipitation and adsorption. The above steps are repeated at least once to make the R value 10-35% to obtain a modified molecular sieve. The R value represents the mass fraction of rare earth elements in the modified molecular sieve as oxides. The modified molecular sieve has β-cage and supercage structures, and the K value is 1-20. The K value represents the ratio of the rare earth element content in the β-cage to the supercage in the modified molecular sieve.

[0034] In this invention, the preparation method of modified molecular sieves can achieve specific rare earth element loading and control the distribution of rare earth elements in β cages and supercages through at least two cross-linking and two baking processes and at least one rare earth oxide precipitation adsorption, thereby improving the lifetime of modified molecular sieves, thereby improving the lifetime of solid acid catalysts, suppressing the occurrence of side reactions, and improving the linearity of the target product.

[0035] In this invention, by controlling the operation steps, conditions and the number of repetitions of each step in steps (1)-(3), the R value and K value in the modified molecular sieve are made to meet the above-mentioned R value of 10-35% and K value of 1-20. In this invention, the preferred range of R value and K value and the determination method have been described in the foregoing content and will not be repeated here.

[0036] Specifically, in this invention, by controlling the conditions, parameters, and number of repetitions of the first ion exchange calcination, the various process parameters work synergistically to allow rare earth elements to migrate into the β cage of the molecular sieve, while simultaneously performing reverse exchange on the rare earth elements in the supercage. Subsequently, a second ion exchange is performed, and by controlling the conditions of the second ion exchange, the element content in the β cage and supercage is regulated. Finally, rare earth oxide precipitation and adsorption are performed, and by controlling the conditions of rare earth oxide precipitation and adsorption, the content of rare earth elements in the molecular sieve is regulated, so that the R value and K value of the modified molecular sieve meet the aforementioned conditions.

[0037] In this invention, there is no particular limitation on the type of molecular sieve in step (1), as long as it meets the requirements for preparing modified molecular sieves. Preferably, in step (1), the molecular sieve is a silica-alumina molecular sieve.

[0038] In a preferred embodiment, the silicon-to-aluminum molar ratio of the molecular sieve in step (1) is 1-50, more preferably 1.5-9. In this invention, it is understood that the silicon-to-aluminum molar ratio refers to the molar ratio of silicon atoms to aluminum atoms.

[0039] In this invention, the silicon-aluminum molar ratio remains essentially unchanged before and after molecular sieve modification, both satisfying the above-mentioned molar ratio range requirements.

[0040] In a preferred embodiment, the molecular sieve in step (1) is in the form of hydrogen and / or ammonium, and more preferably in the form of ammonium.

[0041] In a preferred embodiment, the molecular sieve in step (1) is an X-type molecular sieve and / or a Y-type molecular sieve.

[0042] In this invention, molecular sieves with β-cage and supercage structures are selected as raw materials for modification. The advantage of the supercage structure of molecular sieves, which makes it easier for reactants to come into contact, is utilized to improve the lifespan of the modified molecular sieves.

[0043] In this invention, the types of rare earth elements in steps (1)-(3) have been described above and will not be repeated here.

[0044] In a preferred embodiment, the rare earth element ion exchange liquids in steps (1), (2), and (3) are each independently selected from solutions containing rare earth element compounds.

[0045] In this invention, there is no particular limitation on the type of rare earth element compound, as long as it can provide rare earth element ions. Preferably, the rare earth element compound is selected from at least one of the nitrate, sulfate, and chloride salts of the corresponding rare earth element, and more preferably a nitrate.

[0046] In this invention, the concentration of the rare earth ion exchange solution is not particularly limited. Preferably, the concentration of the rare earth ion exchange solution in steps (1), (2) and (3) is 0.18-1 mol / L, and more preferably 0.35-0.8 mol / L.

[0047] In this invention, it is understood that the concentrations of the rare earth ion exchange liquids in steps (1)-(3) can be the same or different during the preparation of the modified molecular sieve.

[0048] In this invention, there is no particular limitation on the amount of rare earth element ion exchange liquid used. Preferably, the ratio of the mass of the molecular sieve to the volume of the rare earth element ion exchange liquid in step (1) is 150-550 g / L, more preferably 200-400 g / L.

[0049] In this invention, preferably, the first ion exchange in step (1) is carried out under stirring conditions.

[0050] In this invention, the selection range of conditions for the first ion exchange in step (1) is relatively wide. Preferably, the conditions for the first ion exchange in step (1) include: a temperature of 60-120℃, a time of 0.5-1.5h, and a stirring rate of 200-500r / min. More preferably, the temperature is 75-95℃, the time is 0.8-1.2h, and the stirring rate is 300-400r / min.

[0051] In this invention, preferably, after the molecular sieve undergoes the first ion exchange, it is subjected to solid-liquid separation followed by a first drying in step (1). The method of solid-liquid separation is not particularly limited in this invention; for example, filtration may be used. In this invention, the selection range for the first drying conditions is relatively wide. Preferably, the conditions for the first drying include: a temperature of 50-180℃ and a time of 2-10 hours.

[0052] In a preferred embodiment, in step (1), the calcination is carried out under an alkaline atmosphere and a slightly positive pressure.

[0053] In a preferred embodiment, the alkaline atmosphere in step (1) is provided by ammonia. It is understood in this invention that ammonia can rapidly vaporize under calcination conditions, thereby providing an alkaline atmosphere for the calcination process.

[0054] In this invention, the concentration of ammonia water is not particularly limited, as long as an alkaline atmosphere can be provided. Preferably, the concentration of ammonia water in step (1) is 0.05-0.5 mol / L, and more preferably 0.08-0.3 mol / L.

[0055] In this invention, there is no particular limitation on the ammonia water introduction rate. Preferably, compared to 50g of molecular sieve, the ammonia water introduction rate is 0.01-5mL / min, more preferably 0.05-3mL / min. It is understood in this invention that the alkaline atmosphere (ammonia water) introduction rate is proportional to the molecular sieve throughput; for example, as the molecular sieve throughput increases, the alkaline atmosphere (ammonia water) introduction rate can be increased proportionally. Those skilled in the art can select the appropriate rate based on actual needs.

[0056] In this invention, the selection range for the calcination conditions in step (1) is relatively wide. Preferably, the calcination conditions in step (1) include: a temperature of 400-600℃, a time of 0.5-2h, and a pressure of 0.01-0.1MPa; more preferably, a temperature of 450-580℃, a time of 0.8-1.5h, and a pressure of 0.001-0.05MPa, with the pressure measured in gauge pressure. The advantage of this preferred embodiment is that it facilitates the diffusion of rare earth elements into the molecular sieve β cage.

[0057] In this invention, there is no particular limitation on the type of acid in the acid solution described in step (1), and acids conventionally defined in the art are applicable to this invention. Preferably, the acid in the acid solution described in step (1) is selected from inorganic acids and / or organic acids, preferably inorganic acids, and more preferably at least one of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, and boric acid.

[0058] In this invention, the concentration of the acid solution in step (1) is not particularly limited, as long as the pH of the solution is within the range of 1-4. Preferably, the concentration of the acid solution in step (1) is 0.0001-0.1 mol / L, and more preferably 0.001-0.1 mol / L.

[0059] In this invention, the selection range for the acid treatment conditions in step (1) is relatively wide. Preferably, the acid treatment conditions in step (1) include: a temperature of 40-80℃, a time of 0.5-2h, and a stirring rate of 200-500r / min; more preferably, a temperature of 55-75℃, a time of 0.8-1.5h, and a stirring rate of 300-400r / min. In this invention, after the acid treatment in step (1), a second drying is performed following solid-liquid separation. The method of solid-liquid separation in this invention has been described above and will not be repeated here. In this invention, the selection range for the second drying conditions is relatively wide. Preferably, the second drying conditions include: a temperature of 50-180℃ and a time of 2-10h.

[0060] In a preferred embodiment, the repetition of step (1) is 1-3 times, preferably 1-2 times. Under the above preferred conditions, it is beneficial for rare earth elements to fill into the molecular sieve β cage.

[0061] In a preferred embodiment, the ratio of the mass of the first ion exchange product to the volume of the rare earth element ion exchange liquid in step (2) is 200-600 g / L, preferably 300-450 g / L.

[0062] In a preferred embodiment, in step (2), the second ion exchange is carried out under stirring conditions.

[0063] In this invention, the selection range of conditions for the second ion exchange is relatively wide. Preferably, the conditions for the second ion exchange include: a temperature of 80-130℃, a time of 0.5-3h, and a stirring rate of 200-500r / min. More preferably, the temperature is 80-100℃, the time is 0.8-1.2h, and the stirring rate is 300-400r / min.

[0064] In this invention, after the second ion exchange in step (2), solid-liquid separation is performed followed by a third drying. The method of solid-liquid separation in this invention has been described above and will not be repeated here. In this invention, the selection range of the conditions for the third drying is relatively wide. Preferably, the conditions for the third drying include: a temperature of 50-180℃ and a time of 2-10h.

[0065] In a preferred embodiment, the number of repetitions in step (2) is 1-3 times, preferably 1-2 times.

[0066] In a preferred embodiment, the ratio of the mass of the second ion exchange product to the volume of the rare earth element ion exchange liquid in step (3) is 100-400 g / L, preferably 250-350 g / L.

[0067] In this invention, by controlling the conditions and repetition frequency of rare earth oxide precipitation and adsorption in step (3), the B value in the modified molecular sieve meets the following range requirements. In a preferred embodiment, in step (3), the B value is 1.1-1.5, preferably 1.2-1.4, where the B value represents the mass fraction ratio of rare earth elements (calculated as oxides) in the surface phase and bulk phase of the modified molecular sieve. The range of B values ​​and the determination method in this invention have been described above and will not be repeated here.

[0068] In this invention, preferably, the rare earth oxide precipitation and adsorption in step (3) is carried out under alkaline conditions. The advantage of this preferred embodiment is that it promotes the migration of rare earth ions from the supercage into the β-cage.

[0069] In a preferred embodiment, the alkaline conditions in step (3) are provided by an alkaline compound.

[0070] In this invention, there is no particular limitation on the type of alkaline compound. Preferably, the alkaline compound in step (3) is selected from at least one of ammonia, ammonium carbonate and urea, and more preferably ammonia.

[0071] In this invention, there is no particular limitation on the concentration of the alkaline compound, as long as it can adjust the pH of the solution to 8-10. Preferably, the concentration of the alkaline compound in step (3) is 1-4 mol / L.

[0072] In this invention, the selection range of conditions for rare earth oxide precipitation and adsorption is relatively wide. Preferably, the conditions for rare earth oxide precipitation and adsorption include: temperature of 0-50℃, time of 0.2-1.5h, and stirring rate of 200-500r / min; more preferably, temperature of 5-30℃, time of 0.2-0.8h, and stirring rate of 300-400r / min. Under these conditions, the rare earth oxide precipitation and adsorption of the second ion exchange product has the advantage of quantitative adsorption. In this invention, after the rare earth oxide precipitation and adsorption in step (3), solid-liquid separation is performed followed by a fourth drying. The solid-liquid separation method in this invention has been described above and will not be repeated here. In this invention, the selection range of conditions for the fourth drying is relatively wide. Preferably, the conditions for the fourth drying include: temperature of 50-180℃ and time of 2-10h.

[0073] In a preferred embodiment, the number of repetitions in step (3) is 1-3 times, preferably 1-2 times.

[0074] In this invention, a wide range of adhesive types can be selected. Preferably, the adhesive is a heat-resistant inorganic oxide.

[0075] In a preferred embodiment, the binder is selected from at least one of alumina, zirconium oxide, silicon dioxide, and titanium dioxide, and is more preferably alumina.

[0076] In this invention, there is no particular limitation on the preparation method of the solid acid catalyst. The preparation method conventionally defined in the art can be selected, such as the extrusion molding method. Specifically, the preparation method of the solid acid catalyst includes: mixing the modified molecular sieve with a binder and / or its precursor, water, and optionally an extrusion aid and a peptizing agent in the presence of the mixture, molding, and then sequentially performing molding drying and molding calcination.

[0077] In this invention, the types of modified molecular sieves and binders have been described above and will not be repeated here.

[0078] In this invention, preferably, the binder precursor is selected from at least one of oxide sol, aluminum salt, silicate, titanium salt, and zirconium salt. For example, the oxide sol includes at least one of silica sol, titanium sol, and zirconium sol; the aluminum salt is selected from at least one of boehmite, aluminum chloride, and aluminum sulfate; the silicate is at least one of sodium silicate, potassium silicate, and calcium silicate; the titanium salt is selected from titanium sulfate and / or titanium tetrachloride, etc.; and the zirconium salt is zirconium chloride and / or zirconium sulfate.

[0079] In a preferred embodiment, the average particle size of the binder and / or its precursor is 0.005-200 μm, more preferably 30-150 μm.

[0080] In a preferred embodiment, the weight ratio of the modified molecular sieve to the binder and / or its precursor, on a dry basis, is 99:1-20:80, preferably 95:5-25:75, and more preferably 90:10-50:50.

[0081] In this invention, "on a dry basis" is defined as the mass of a unit mass of catalyst after calcination at 600°C for 3 hours.

[0082] In this invention, there is no particular limitation on the type of extrusion aid; any extrusion aid conventionally defined in the art is applicable to this invention. Preferably, the extrusion aid is selected from at least one of guar gum powder, cellulose, and starch.

[0083] In this invention, there is no particular limitation on the amount of extrusion aid. Preferably, the amount of extrusion aid is 0-10 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor, and more preferably 2-6 wt%.

[0084] In this invention, there is no particular limitation on the type of adhesive solvent; adhesive solvents conventionally defined in the art are applicable to this invention. Preferably, the adhesive solvent is selected from at least one of citric acid, nitric acid, and phosphoric acid.

[0085] In this invention, there is no particular limitation on the amount of adhesive solvent used. Preferably, the amount of adhesive solvent used is 0-12 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor, and more preferably 2-6 wt%.

[0086] In this invention, the amount of water used is not particularly limited, as long as it is sufficient to ensure uniform mixing of the modified molecular sieve, binder, extrusion aid, and adhesive. Preferably, the amount of water used is 50-200 wt% of the total dry weight of the modified molecular sieve, binder, and / or its precursor, and more preferably 50-100 wt%.

[0087] In this invention, the molding and drying conditions are such that the dry basis weight of the mixed molded article after drying is 50-90 wt%, preferably 60-80 wt%.

[0088] In a preferred embodiment, the molding and drying conditions include a temperature of 60-200°C and a time of 1-12 hours.

[0089] In this invention, the selection range for the molding and calcining conditions is relatively wide. Preferably, the molding and calcining conditions include: a temperature of 350-650℃ and a time of 0.5-8h; more preferably, a temperature of 420-580℃ and a time of 2-6h.

[0090] In a preferred embodiment, the straight-chain olefin is a mixture in which the unsaturated bond is located on the top carbon atom or one of the middle carbon atoms of the straight-chain olefin.

[0091] In a preferred embodiment, the straight-chain olefin is a C6-C25 linear olefin, more preferably a C8-C14 linear olefin, and even more preferably a C9-C13 linear olefin.

[0092] In a preferred embodiment, the aromatic hydrocarbon is selected from at least one of benzene, toluene, and ethylbenzene, preferably benzene.

[0093] In a preferred embodiment, the alkylation reaction is a liquid-phase reaction. The advantage of this preferred embodiment is that it increases the contact time between the reactants and the catalyst, allowing for a more complete reaction. In this invention, it is understood that a liquid-phase alkylation reaction means that the alkylation reaction is carried out in a liquid phase, and the pressure is always sufficient to ensure that the reaction proceeds in a single liquid phase. In this invention, a single liquid phase refers to the fact that all reactants are in a liquid phase, and the reaction conditions are such that the reactants do not vaporize during the reaction.

[0094] In a preferred embodiment, the alkylation conditions include: a temperature of 70-270°C, a pressure of 0.2-8 MPa, a molar ratio of aromatics to straight-chain olefins of 6:1-85:1, and a feed straight-chain olefin mass hourly space velocity of 0.05-4.5 h⁻¹. -1 .

[0095] In a preferred embodiment, the alkylation conditions include: a temperature of 90-190°C, a pressure of 1.5-3.8 MPa, a molar ratio of straight-chain olefin to aromatic hydrocarbon of 8:1-62:1, and a feed straight-chain olefin mass hourly space velocity of 0.2-2.8 h⁻¹. -1 .

[0096] According to the method of the present invention, contacting linear olefins and aromatics in the presence of a solid acid catalyst can improve the catalyst cycle life, the selectivity of the target product, and the linearity of the target product.

[0097] The present invention will be described in detail below through examples. In the following examples, unless otherwise specified, all raw materials used are commercially available.

[0098] Example 1

[0099] Preparation of modified molecular sieves

[0100] (1) Prepare a 0.5 mol / L lanthanum nitrate solution, then mix it with NH4Y molecular sieve (silicon-aluminum molar ratio of 3.13) and stir evenly. Heat and stir at 85℃ for 1 h at a stirring rate of 400 r / min. The mass ratio of NH4Y molecular sieve to lanthanum nitrate solution is 350 g / L. After heating, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0101] (2) The filter cake was roasted at high temperature for 1 hour. The roasting conditions were: temperature 560℃, pressure 0.02MPa, and 0.1mol / L ammonia water was introduced at a flow rate of 0.1mL / min.

[0102] (3) The calcined sample was mixed with 0.005 mol / L HNO3 solution and stirred evenly. The mixture was heated and stirred at 75°C for 1 h at a stirring rate of 400 r / min. The mixture was then filtered, the filter cake was thoroughly washed, and the filter cake was dried at 110°C for 4 h.

[0103] (4) Repeat steps (1)-(3) once to obtain the first ion exchange product.

[0104] (5) Mix the sample with 0.5 mol / L lanthanum nitrate solution and stir evenly. Heat and stir at 85°C for 1 h at a stirring rate of 400 r / min. The mass ratio of the first ion exchange product to the volume of the lanthanum nitrate solution is 300 g / L. After heating, filter, wash the filter cake and dry at 110°C for 4 h.

[0105] (6) Repeat step (5) once to obtain the second ion exchange product.

[0106] (7) Mix the filter cake with 0.5 mol / L lanthanum nitrate solution, and adjust the pH of the slurry to 9 with 2 mol / L ammonia water. Stir at 25℃ for 0.4 h with a stirring rate of 400 r / min. After stirring, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0107] (8) Repeat step (7) once.

[0108] (9) The molecular sieve prepared above is numbered S1.

[0109] XRD, XRF, and XPS analyses were performed on the modified molecular sieve S1 to obtain the mass fraction of La element in the modified molecular sieve as oxides, the content ratio of La element in the β cage and the supercage of the modified molecular sieve, the mass fraction ratio of La element in the surface phase and the bulk phase of the modified molecular sieve as oxides, and the silica-alumina molar ratio of the modified molecular sieve. The results are shown in Table 1.

[0110] In Table 1, the mass fraction of La element loaded in the molecular sieve as oxides is represented by the R value, the ratio of La element content in the β cage to the supercage of the molecular sieve is represented by the K value, and the ratio of the mass fraction of La element in the surface phase to the bulk phase of the molecular sieve as oxides is represented by the B value.

[0111] Preparation of solid acid catalysts:

[0112] Modified molecular sieve sample S1 was mixed with boehmite (average particle size 100 μm, Sinopec Catalyst Co., Ltd.) at a dry weight ratio of 80:20. 3 wt% guar gum powder and 3 wt% nitric acid were added respectively (based on the total dry weight of modified molecular sieve and boehmite). Based on the dry weight of modified molecular sieve and boehmite, 100 wt% deionized water of the dry weight of modified molecular sieve and boehmite was added. After mixing evenly, the mixture was extruded and dried at 110℃ for 4 h to make the dry weight of the dried mixture 65 wt%. Then, it was calcined in air at 550℃ for 4 h to obtain a solid acid catalyst.

[0113] Preparation of straight-chain alkylbenzenes:

[0114] The alkylation reaction of benzene with 1-dodecene was carried out at 130 °C and 2.5 MPa, with a feed space velocity of 0.708 h⁻¹ for 1-dodecene. -1 The molar ratio of benzene to 1-dodecene was 10. Under these reaction conditions, the conversion rate of 1-dodecene, the linearity of the product, and the selectivity for isoolefins are shown in Table 2. The trend of 1-dodecene conversion rate is shown in the graph below. Figure 1 As shown in the figure, the trend of product linearity is as follows: Figure 2 As shown.

[0115] Conversion rate of 1-dodecene (%) = (Amount of 1-dodecene before reaction - Amount of 1-dodecene after reaction) / Amount of 1-dodecene before reaction × 100%.

[0116] Isoalkanes selectivity (%) = Amount of isoalkanes after reaction / Amount of all reaction products × 100%;

[0117] Straight-chain degree (%) = Amount of straight-chain alkylbenzene after reaction / Amount of monoalkylbenzene after reaction × 100%.

[0118] Example 2

[0119] Preparation of modified molecular sieves:

[0120] (1) Prepare a 0.8 mol / L lanthanum nitrate solution, then mix it with NH4Y molecular sieve (silicon-aluminum molar ratio of 3.13) and stir evenly. Heat and stir at 95℃ for 1.2 h at a stirring rate of 400 r / min. The mass ratio of NH4Y molecular sieve to lanthanum nitrate solution is 350 g / L. After heating, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0121] (2) The filter cake was roasted at high temperature for 1.5 hours. The roasting conditions were: temperature 580℃, pressure 0.05MPa, and 0.3mol / L ammonia water was introduced at a flow rate of 3mL / min.

[0122] (3) The calcined sample was mixed with 0.005 mol / L HNO3 solution and stirred evenly. The mixture was heated and stirred at 75°C for 1 h at a stirring rate of 400 r / min. The mixture was then filtered, the filter cake was thoroughly washed, and the filter cake was dried at 110°C for 4 h.

[0123] (4) Repeat steps (1)-(3) once to obtain the first ion exchange product.

[0124] (5) Mix the sample with 0.8 mol / L lanthanum nitrate solution and stir evenly. Heat and stir at 100℃ for 1.2 h at a stirring rate of 400 r / min. The mass ratio of the first ion exchange product to the volume of the lanthanum nitrate solution is 300 g / L. After heating, filter, wash the filter cake and dry at 110℃ for 4 h.

[0125] (6) Repeat step (5) once to obtain the second ion exchange product.

[0126] (7) Mix the filter cake with 0.5 mol / L lanthanum nitrate solution, and adjust the pH of the slurry to 9 with 2 mol / L ammonia water. Stir at 30℃ for 0.8 h with a stirring rate of 400 r / min. After stirring, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0127] (8) Repeat step (7) once.

[0128] (9) The molecular sieve prepared above is numbered S2.

[0129] Preparation of solid acid catalysts:

[0130] Modified molecular sieve sample S2 and pseudoboehmite (average particle size 100 μm, Sinopec Catalyst Co., Ltd.) were mixed at a dry weight ratio of 90:10. 6 wt% of guar gum powder and 6 wt% of nitric acid were added respectively (based on the total dry weight of modified molecular sieve and pseudoboehmite). Based on the dry weight of modified molecular sieve and pseudoboehmite, 100 wt% of deionized water was added. After mixing evenly, the mixture was extruded and dried at 110℃ for 4 h to make the dry weight of the dried mixture 65 wt%. Then, it was calcined in air at 580℃ for 6 h to obtain a solid acid catalyst.

[0131] Preparation of straight-chain alkylbenzenes:

[0132] In the preparation of straight-chain alkylbenzenes, the reaction temperature was replaced with 200℃, the pressure with 3.8 MPa, the molar ratio of benzene to 1-dodecene with 60, and the feed space velocity of the straight-chain olefin was 2.8 h⁻¹. -1 .

[0133] Example 3

[0134] Preparation of modified molecular sieves:

[0135] (1) Prepare a 0.35 mol / L lanthanum nitrate solution, then mix it with NH4Y molecular sieve (silicon-aluminum molar ratio of 3.13) and stir evenly. Heat and stir at 75℃ for 0.8 h at a stirring rate of 400 r / min. The mass ratio of NH4Y molecular sieve to lanthanum nitrate solution is 350 g / L. After heating, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0136] (2) The filter cake was roasted at high temperature for 0.8h. The roasting conditions were: temperature 450℃, pressure 0.01MPa, and 0.08mol / L ammonia water was introduced at a flow rate of 0.05mL / min.

[0137] (3) The calcined sample was mixed with 0.005 mol / L HNO3 solution and stirred evenly. The mixture was heated and stirred at 75°C for 1 h at a stirring rate of 400 r / min. The mixture was then filtered, the filter cake was thoroughly washed, and the filter cake was dried at 110°C for 4 h.

[0138] (4) Repeat steps (1)-(3) once to obtain the first ion exchange product.

[0139] (5) Mix the sample with 0.35 mol / L lanthanum nitrate solution and stir evenly. Heat and stir at 80°C for 0.8 h at a stirring rate of 400 r / min. The mass ratio of the first ion exchange product to the volume of the lanthanum nitrate solution is 300 g / L. After heating, filter, wash the filter cake and dry at 110°C for 4 h.

[0140] (6) Repeat step (5) once to obtain the second ion exchange product.

[0141] (7) Mix the filter cake with 0.5 mol / L lanthanum nitrate solution, and adjust the pH of the slurry to 9 with 2 mol / L ammonia water. Stir at 5℃ for 0.2 h with a stirring rate of 400 r / min. After stirring, filter the slurry and dry the filter cake at 110℃ for 4 h.

[0142] (8) Repeat step (7) once.

[0143] (9) The molecular sieve prepared above is numbered S3.

[0144] Preparation of solid acid catalysts:

[0145] Modified molecular sieve sample S3 and pseudoboehmite (average particle size 100 μm, Sinopec Catalyst Co., Ltd.) were mixed at a dry weight ratio of 50:50. 2 wt% of guar gum powder and 2 wt% of nitric acid were added respectively (based on the total dry weight of the modified molecular sieve and pseudoboehmite). Based on the dry weight of the modified molecular sieve and pseudoboehmite, 50 wt% of deionized water was added. After mixing evenly, the mixture was extruded and dried at 110 °C for 4 h to obtain a dry weight of 65 wt% for the dried mixture. Then, it was calcined in air at 420 °C for 2 h to obtain a solid acid catalyst.

[0146] Preparation of straight-chain alkylbenzenes:

[0147] In the preparation of straight-chain alkylbenzenes, the reaction temperature was replaced with 70℃, the pressure with 1.5 MPa, the molar ratio of benzene to 1-dodecene with 8, and the feed mass hourly space velocity of the straight-chain olefin was 0.2 h⁻¹. -1 .

[0148] Example 4

[0149] The method described in Example 1 is followed, except that the concentration of the lanthanum nitrate solution in step (1) and step (5) is replaced with 0.2 mol / L during the preparation of the modified molecular sieve. The molecular sieve prepared above is designated as S4.

[0150] Example 5

[0151] The method described in Example 1 is followed, except that in the preparation of the modified molecular sieve, the heating temperature in step (1) is replaced with 70°C and the stirring time is replaced with 0.6 h, and the heating temperature in step (5) is replaced with 80°C and the stirring time is replaced with 0.6 h. The molecular sieve prepared above is designated as S5.

[0152] Example 6

[0153] The method described in Example 1 was followed, except that the concentration of the HNO3 solution in step (3) was replaced with 0.0001 mol / L during the preparation of the modified molecular sieve. The molecular sieve prepared above was designated as S6.

[0154] Example 7

[0155] The method described in Example 1 is followed, except that the calcination temperature in step (2) is replaced with 420°C during the preparation of the modified molecular sieve. The molecular sieve prepared above is designated as S7.

[0156] Example 8

[0157] The method described in Example 1 is followed, except that in the preparation of the modified molecular sieve, the lanthanum nitrate solution in step (1) is replaced with a yttrium nitrate solution, the lanthanum nitrate solution in step (5) is replaced with a yttrium nitrate solution, and the lanthanum nitrate solution in step (7) is replaced with a yttrium nitrate solution. The molecular sieve prepared above is designated as S8.

[0158] Example 9

[0159] The method described in Example 1 was followed, except that in the preparation of the modified molecular sieve, the 0.1 mol / L ammonia water in step (2) was replaced with air as the calcination atmosphere. The molecular sieve prepared above was designated as S9.

[0160] Example 10

[0161] The method is the same as in Example 1, except that in the preparation of linear alkylbenzene, the raw material 1-dodecene is replaced with 1-eicosene.

[0162] Example 11

[0163] The method described in Example 1 is followed, except that the reaction temperature in the preparation of linear alkylbenzenes is replaced with 220°C, the pressure is replaced with 6 MPa, the molar ratio of benzene to 1-dodecene is replaced with 75, and the feed mass hourly space velocity of the linear olefin is 0.1 h⁻¹. -1 .

[0164] Comparative Example 1

[0165] The method of Example 1 was followed, except that the untreated NH4Y molecular sieve from Example 1 was used. The resulting comparative molecular sieve was designated CS1.

[0166] Comparative Example 2

[0167] The method described in Example 1 is followed, except that in the preparation of the modified molecular sieve, the concentration of the lanthanum nitrate solution used in steps (1), (5), and (7) is 0.15 mol / L. The resulting comparative molecular sieve is designated CS2.

[0168] Comparative Example 3

[0169] The method described in Example 1 was followed, except that the concentration of the lanthanum nitrate solution used in steps (1), (5), and (7) of the modified molecular sieve preparation process was 1.3 mol / L. The resulting comparative molecular sieve was designated CS3.

[0170] Comparative Example 4

[0171] The method is the same as in Example 1, except that in the preparation of the modified molecular sieve, the mass ratio of NH4Y molecular sieve to lanthanum nitrate solution in step (1) is 150 g / L, and the mass ratio of NH4Y molecular sieve to lanthanum nitrate solution in step (5) is 100 g / L.

[0172] Comparative Example 5

[0173] The method described in Example 1 was followed, except that steps (4) and (6) were omitted during the preparation of the modified molecular sieve. The resulting comparative molecular sieve was designated CS5.

[0174] Table 1

[0175]

[0176]

[0177] Table 2

[0178]

[0179]

[0180] Note: In Table 2, "-" indicates that the solid acid catalyst has been deactivated.

[0181] As can be seen from Table 2, when the R value, K value, and B value of the modified molecular sieve are within the protection range of this invention, the solid acid catalyst prepared using it has a significant improvement in the linearity of the product and can effectively reduce the selectivity of isomeric olefins.

[0182] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing a straight-chain alkylbenzene, characterized in that, The method includes: reacting a straight-chain olefin with an aromatic hydrocarbon in the presence of a solid acid catalyst under alkylation reaction conditions; The solid acid catalyst comprises a modified molecular sieve and a binder. The modified molecular sieve includes a molecular sieve and rare earth elements. The modified molecular sieve has β-cage and supercage structures. The R value of the modified molecular sieve is 16-35%, and the K value is 1-20. The R value represents the mass fraction of rare earth elements in the modified molecular sieve as oxides, and the K value represents the ratio of the rare earth element content in the β-cage to the content in the supercage of the modified molecular sieve. The modified molecular sieve has a B value of 1.2-1.4, where the B value represents the mass fraction ratio of rare earth elements (calculated as oxides) in the surface phase and bulk phase of the modified molecular sieve. The rare earth elements are selected from Sc, Y, and non-radioactive lanthanides.

2. The method according to claim 1, wherein, The modified molecular sieve has an R value of 16-28%.

3. The method according to claim 1 or 2, wherein, The K value of the modified molecular sieve is 2-8.

4. The method according to claim 1 or 2, wherein, The modified molecular sieve is a silica-alumina molecular sieve.

5. The method according to claim 4, wherein, The modified molecular sieve has a silicon-to-aluminum molar ratio of 1-50.

6. The method according to claim 5, wherein, The modified molecular sieve has a silicon-to-aluminum molar ratio of 1.5-9.

7. The method according to claim 1 or 2, wherein, The rare earth element is selected from at least one of Sc, Y, La, Ce, Pr, Nd, Sm and Yb.

8. The method according to claim 7, wherein, The rare earth elements are La and / or Ce.

9. The method according to claim 1 or 2, wherein, The preparation method of the modified molecular sieve includes: (1) Place the molecular sieve in a rare earth element ion exchange solution, perform the first ion exchange, and then calcine it. Treat the calcined product with acid in an acid solution. Repeat the above steps at least once to obtain the first ion exchange product. (2) Place the first ion exchange product in a rare earth element ion exchange solution for a second ion exchange, and repeat the above steps at least once to obtain the second ion exchange product. (3) Place the second ion exchange product in a rare earth element ion exchange solution for rare earth oxide precipitation and adsorption, and repeat the above steps at least once to obtain a modified molecular sieve.

10. The method according to claim 9, wherein, In step (1), the molecular sieve is a silica-alumina molecular sieve.

11. The method according to claim 10, wherein, The silicon-aluminum molar ratio of the molecular sieve in step (1) is 1-50.

12. The method according to claim 11, wherein, The silicon-aluminum molar ratio of the molecular sieve in step (1) is 1.5-9.

13. The method according to claim 9, wherein, The molecular sieve in step (1) is of the ammonium type and / or hydrogen type.

14. The method according to claim 13, wherein, The molecular sieve in step (1) is of the ammonium type.

15. The method according to claim 10, wherein, The molecular sieve in step (1) is an X-type molecular sieve and / or a Y-type molecular sieve.

16. The method according to claim 9, wherein, In steps (1), (2), and (3), the rare earth element ion exchange solutions are each independently selected from solutions containing rare earth element compounds.

17. The method according to claim 16, wherein, The rare earth element compound is selected from at least one of the nitrate, sulfate and chloride salts of the corresponding rare earth element.

18. The method according to claim 9, wherein, The concentration of the rare earth element ion exchange solution in steps (1), (2) and (3) is 0.18-1 mol / L.

19. The method according to claim 9, wherein, The ratio of the mass of the molecular sieve to the volume of the rare earth element ion exchange liquid in step (1) is 150-550 g / L.

20. The method according to claim 19, wherein, The ratio of the mass of the molecular sieve to the volume of the rare earth element ion exchange liquid in step (1) is 200-400 g / L.

21. The method according to claim 9, wherein, Step (1) The first ion exchange is carried out under stirring conditions.

22. The method according to claim 9, wherein, Step (1) The conditions for the first ion exchange include: temperature of 60-120℃, time of 0.5-1.5h, and stirring rate of 200-500r / min.

23. The method according to claim 22, wherein, Step (1) The conditions for the first ion exchange include: temperature of 75-95℃, time of 0.8-1.2h, and stirring rate of 300-400r / min.

24. The method according to claim 9, wherein, In step (1), the calcination is carried out under alkaline atmosphere and slightly positive pressure conditions.

25. The method according to claim 24, wherein, The alkaline atmosphere in step (1) is provided by ammonia.

26. The method of claim 25, wherein, The concentration of ammonia in step (1) is 0.05-0.5 mol / L.

27. The method according to claim 9, wherein, In step (1), the calcination conditions include: a temperature of 400-600℃, a time of 0.5-2h, and a pressure of 0.01-0.1MPa, with the pressure measured by a gauge.

28. The method according to claim 27, wherein, In step (1), the calcination conditions include: a temperature of 450-580℃, a time of 0.8-1.5h, and a pressure of 0.01-0.05MPa.

29. The method according to claim 9, wherein, The acid in the acid solution in step (1) is selected from inorganic acids and / or organic acids.

30. The method according to claim 29, wherein, The acid in the acid solution in step (1) is an inorganic acid.

31. The method according to claim 30, wherein, The acid in the acid solution in step (1) is selected from at least one of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid and boric acid.

32. The method according to claim 9, wherein, The concentration of the acid solution in step (1) is 0.0001-0.1 mol / L.

33. The method according to claim 9, wherein, The acid treatment conditions in step (1) include: a temperature of 40-80℃, a time of 0.5-2h, and a stirring rate of 200-500r / min.

34. The method according to claim 33, wherein, The acid treatment conditions in step (1) include: a temperature of 55-75℃, a time of 0.8-1.5h, and a stirring rate of 300-400r / min.

35. The method according to claim 9, wherein, The number of repetitions in step (1) is 1-3 times.

36. The method according to claim 35, wherein, The number of repetitions in step (1) is 1-2 times.

37. The method according to claim 9, wherein, Step (2) The ratio of the mass of the first ion exchange product to the volume of the rare earth element ion exchange liquid is 200-600 g / L.

38. The method according to claim 37, wherein, Step (2) The ratio of the mass of the first ion exchange product to the volume of the rare earth element ion exchange liquid is 300-450 g / L.

39. The method according to claim 9, wherein, In step (2), the second ion exchange is carried out under stirring conditions.

40. The method according to claim 9, wherein, The conditions for the second ion exchange include: a temperature of 80-130℃, a time of 0.5-3h, and a stirring rate of 200-500r / min.

41. The method according to claim 40, wherein, The conditions for the second ion exchange include: a temperature of 80-100℃, a time of 0.8-1.2h, and a stirring rate of 300-400r / min.

42. The method according to claim 9, wherein, The number of repetitions in step (2) is 1-3 times.

43. The method according to claim 42, wherein, The number of repetitions in step (2) is 1-2 times.

44. The method according to claim 9, wherein, In step (3), the ratio of the mass of the second ion exchange product to the volume of the rare earth element ion exchange liquid is 100-400 g / L.

45. The method according to claim 44, wherein, In step (3), the ratio of the mass of the second ion exchange product to the volume of the rare earth element ion exchange liquid is 250-350 g / L.

46. ​​The method according to claim 9, wherein, The rare earth oxide precipitation and adsorption in step (3) are carried out under alkaline conditions.

47. The method according to claim 46, wherein, The alkaline conditions described in step (3) are provided by an alkaline compound.

48. The method according to claim 47, wherein, The alkaline compound in step (3) is selected from at least one of ammonia, ammonium carbonate and urea.

49. The method according to claim 48, wherein, The concentration of the alkaline compound in step (3) is 1-4 mol / L.

50. The method according to claim 9, wherein, The conditions for rare earth oxide precipitation and adsorption in step (3) include: temperature of 0-50℃, time of 0.2-1.5h, and stirring rate of 200-500r / min.

51. The method according to claim 50, wherein, The conditions for the rare earth oxide precipitation and adsorption in step (3) include: temperature of 5-30℃, time of 0.2-0.8h, and stirring rate of 300-400r / min.

52. The method according to claim 9, wherein, The number of repetitions in step (3) is 1-3 times.

53. The method according to claim 52, wherein, The number of repetitions in step (3) is 1-2 times.

54. The method according to claim 1 or 2, wherein, The adhesive is a heat-resistant inorganic oxide.

55. The method according to claim 54, wherein, The binder is selected from at least one of alumina, zirconium oxide, silicon dioxide, and titanium dioxide.

56. The method according to claim 55, wherein, The adhesive is aluminum oxide.

57. The method according to claim 1 or 2, wherein, The preparation method of the solid acid catalyst includes: mixing the modified molecular sieve with a binder and / or its precursor, water, and optionally an extrusion aid and a peptizing agent in the presence of the mixture, molding, and then sequentially performing molding drying and molding calcination.

58. The method according to claim 57, wherein, On a dry basis, the weight ratio of the modified molecular sieve to the binder and / or its precursor is 99:1-20:

80.

59. The method according to claim 58, wherein, On a dry basis, the weight ratio of the modified molecular sieve to the binder and / or its precursor is 95:5-25:

75.

60. The method according to claim 59, wherein, On a dry basis, the weight ratio of the modified molecular sieve to the binder and / or its precursor is 90:10 to 50:

50.

61. The method according to claim 57, wherein, The extrusion aid is selected from at least one of guar gum powder, cellulose, and starch.

62. The method according to claim 57, wherein, The amount of the extrusion aid is 0-10 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

63. The method according to claim 62, wherein, The amount of the extrusion aid is 2-6 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

64. The method according to claim 57, wherein, The colloidal solvent is selected from at least one of citric acid, nitric acid, and phosphoric acid.

65. The method according to claim 57, wherein, The amount of the adhesive solvent is 0-12 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

66. The method according to claim 65, wherein, The amount of the adhesive solvent is 2-6 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

67. The method of claim 57, wherein, The amount of water used is 50-200 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

68. The method according to claim 67, wherein, The amount of water used is 50-100 wt% of the total dry weight of the modified molecular sieve, binder and / or its precursor.

69. The method according to claim 57, wherein, The drying conditions for molding include: a temperature of 60-200℃ and a time of 1-12h.

70. The method of claim 57, wherein, The conditions for molding and baking include: a temperature of 350-650℃ and a time of 0.5-8h.

71. The method according to claim 70, wherein, The conditions for molding and calcination include: a temperature of 420-580℃ and a time of 2-6 hours.

72. The method according to claim 1 or 2, wherein, The straight-chain olefin is a mixture in which the unsaturated bond is located on the top carbon atom or one of the middle carbon atoms of the straight-chain olefin.

73. The method according to claim 72, wherein, The straight-chain olefin is a linear olefin of C6-C25.

74. The method according to claim 73, wherein, The straight-chain olefin is a C8-C14 linear olefin.

75. The method according to claim 74, wherein, The straight-chain olefin is a C9-C13 linear olefin.

76. The method according to claim 75, wherein, The aromatic hydrocarbon is selected from at least one of benzene, toluene, and ethylbenzene.

77. The method according to claim 76, wherein, The aromatic hydrocarbon is benzene.

78. The method according to claim 1 or 2, wherein, The alkylation reaction is a liquid-phase reaction.

79. The method according to claim 1 or 2, wherein, The alkylation conditions include: a temperature of 70-270℃, a pressure of 0.2-8 MPa, a molar ratio of aromatics to straight-chain olefins of 6:1-85:1, and a feed straight-chain olefin mass hourly space velocity of 0.05-4.5 h⁻¹. -1 .

80. The method according to claim 79, wherein, The alkylation conditions include: a temperature of 90-190℃, a pressure of 1.5-3.8 MPa, a molar ratio of aromatics to straight-chain olefins of 8:1-62:1, and a feed straight-chain olefin mass hourly space velocity of 0.2-2.8 h⁻¹. -1 .

Citation Information

Patent Citations

  • Layered zeolitic catalyst for improved linearity in detergent alkylation

    CN101861290A

  • Rare earth exchanged catalyst for use in detergent alkylation

    CN102655932A

  • Modified Y type molecular sieve and preparation method thereof

    CN103130240A