Preparation method of sulfonated polyether ether ketone-based composite proton exchange membrane and application thereof

The composite proton exchange membrane prepared by sulfonated polyether ether ketone and dopamine hydrochloride composite membrane and modified with polytetrafluoroethylene dispersion emulsion improves the proton conductivity and enhances the mechanical and thermal stability, thus solving the problem of membrane performance degradation in the prior art.

CN117659462BActive Publication Date: 2026-11-20SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311401149.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2026-11-20
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

While existing sulfonated polyether ether ketone proton exchange membranes improve proton conductivity, they also increase water absorption and swelling, deteriorate mechanical properties, increase vanadium ion permeation, and decrease ion selectivity.

Method used

A composite proton exchange membrane was formed by using sulfonated polyether ether ketone and dopamine hydrochloride, and modified by polytetrafluoroethylene dispersion emulsion. Polytetrafluoroethylene nanoparticles were used to improve the mechanical and thermal stability of the membrane, while also promoting the improvement of proton conductivity.

Benefits of technology

While enhancing ion selectivity, it also improves proton conductivity, enhances the mechanical and thermal stability of the membrane, and solves the performance degradation problem caused by the increase of sulfonic acid groups.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117659462B_ABST
    Figure CN117659462B_ABST
Patent Text Reader

Abstract

The application provides a preparation method of a sulfonated polyether ether ketone-based composite proton exchange membrane and application thereof, and comprises the following steps: adding sulfonated polyether ether ketone into an organic solvent to obtain a homogeneous solution through ultrasonic treatment; laying a film of the homogeneous solution to obtain a sulfonated polyether ether ketone membrane; immersing the sulfonated polyether ether ketone membrane into a buffer solution, and adding dopamine hydrochloride to prepare a composite membrane of the sulfonated polyether ether ketone and the dopamine hydrochloride; diluting polytetrafluoroethylene emulsion with the buffer solution, and uniformly dispersing the polytetrafluoroethylene emulsion through ultrasonic treatment to prepare a polytetrafluoroethylene dispersion emulsion; immersing the composite membrane of the sulfonated polyether ether ketone and the dopamine hydrochloride into the polytetrafluoroethylene dispersion emulsion, adding dopamine hydrochloride, and taking out and drying to obtain the sulfonated polyether ether ketone-based composite proton exchange membrane. The composite proton exchange membrane prepared by the application can enhance ion selectivity and promote the improvement of proton conductivity, and can avoid the problem that ion selectivity and proton conductivity are difficult to be simultaneously improved due to sulfonic acid groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of proton exchange membranes, specifically relating to a method for preparing a sulfonated polyether ether ketone-based composite proton exchange membrane and its application. Background Technology

[0002] Proton exchange membranes are a key component of vanadium redox flow batteries (VRFBs), and perfluorosulfonic acid (PFSA) membranes are widely used in commercial flow battery systems due to their high proton conductivity and excellent chemical and mechanical stability. However, their high cost ($500 / m2) and high vanadium ion crosslinking have limited the large-scale application of VRFBs to some extent.

[0003] Sulfonated polyether ether ketone (SPEEK) has become a promising alternative to PFSA due to its low cost, simple production and processing, high stability and ion selectivity. However, the proton conductivity of SPEEK is closely related to its degree of sulfonation. The higher the degree of sulfonation, the more sulfonic acid groups (-SO3H) are present in the membrane, and the membrane exhibits higher proton conductivity and ion exchange capacity.

[0004] However, as the number of sulfonic acid groups in the membrane increases, the membrane's water absorption and swelling also increase, its mechanical properties deteriorate, and at the same time, vanadium ion permeation increases, resulting in decreased ion selectivity. Summary of the Invention

[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.

[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a sulfonated polyether ether ketone-based composite proton exchange membrane.

[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing a sulfonated polyether ether ketone-based composite proton exchange membrane, comprising,

[0009] Sulfonated polyether ether ketone is added to an organic solvent and ultrasonicated to obtain a homogeneous solution;

[0010] A sulfonated polyetheretherketone membrane was obtained by coating a homogeneous solution.

[0011] Sulfonated polyether ether ketone membrane was immersed in buffer solution, and dopamine hydrochloride was added to prepare a composite membrane of sulfonated polyether ether ketone and dopamine hydrochloride.

[0012] The polytetrafluoroethylene emulsion was diluted with buffer solution and ultrasonically dispersed evenly to obtain a polytetrafluoroethylene dispersion emulsion.

[0013] The composite membrane of sulfonated polyether ether ketone and dopamine hydrochloride was completely immersed in polytetrafluoroethylene dispersion emulsion, dopamine hydrochloride was added, and the reaction was continued for 60-90 minutes. After drying, the sulfonated polyether ether ketone-based composite proton exchange membrane was obtained.

[0014] As a preferred embodiment of the preparation method described in this invention, the sulfonated polyether ether ketone is added to an organic solvent, wherein the organic solvent includes dimethylformamide, and the ratio of sulfonated polyether ether ketone to organic solvent is 1-4 g: 10-20 mL.

[0015] In a preferred embodiment of the preparation method described in this invention, the homogenized solution is obtained by ultrasound, wherein the ultrasound power is 200-300W.

[0016] As a preferred embodiment of the preparation method described in this invention, the step of obtaining a sulfonated polyetheretherketone membrane by coating a homogeneous solution includes:

[0017] The homogenized solution was poured onto a clean glass plate and allowed to stand at room temperature for 20–24 hours until the membrane was set. The set membrane was then transferred to an oven and dried at 60–80°C for 10–14 hours to obtain a sulfonated polyether ether ketone membrane.

[0018] As a preferred embodiment of the preparation method described in this invention, the sulfonated polyether ether ketone membrane is immersed in a buffer solution, and dopamine hydrochloride is added. The buffer solution includes Tris-HCl buffer solution with a pH of 8.5, and the concentration of dopamine hydrochloride in the buffer solution is 1–1.5 g / L.

[0019] As a preferred embodiment of the preparation method described in this invention, the composite membrane of sulfonated polyether ether ketone and dopamine hydrochloride has a two-layer structure, consisting of a sulfonated polyether ether ketone layer and a dopamine hydrochloride layer, with a thickness ratio of 80-100 μm: 20-50 nm between the two layers.

[0020] In a preferred embodiment of the preparation method described in this invention, the polytetrafluoroethylene dispersion emulsion is prepared using Tris-HCl buffer as the solvent, and the mass-to-volume ratio of polytetrafluoroethylene to the buffer is 0.5–2.5 g: 20–50 mL.

[0021] As a preferred embodiment of the preparation method of the present invention, wherein: the composite film of sulfonated polyether ether ketone and dopamine hydrochloride is completely immersed in polytetrafluoroethylene dispersion emulsion, and dopamine hydrochloride is added, wherein the concentration of dopamine hydrochloride is 1.5 g / L, and the volume ratio of polytetrafluoroethylene dispersion emulsion to dopamine hydrochloride is 1:1.

[0022] As a preferred embodiment of the preparation method described in this invention, the sulfonated polyether ether ketone-based composite proton exchange membrane has a two-layer structure with a thickness ratio of 80-100 μm: 200-250 nm.

[0023] Another objective of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a sulfonated polyether ether ketone-based composite proton exchange membrane, and to apply the sulfonated polyether ether ketone-based composite proton exchange membrane to an all-vanadium redox flow battery.

[0024] Beneficial effects of this invention:

[0025] This invention provides a method for preparing a sulfonated polyether ether ketone (PEEK) composite proton exchange membrane. The resulting composite proton exchange membrane enhances ion selectivity and also improves proton conductivity, avoiding the problem of simultaneously improving ion selectivity and proton conductivity caused by sulfonate groups. Furthermore, polytetrafluoroethylene (PTFE) nanoparticles have extremely strong stability. This invention uses PTFE nanoparticles to modify the sulfonated PEEK membrane, which also significantly improves the mechanical and thermal stability of the composite membrane. Attached Figure Description

[0026] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:

[0027] Figure 1 This is a diagram of the finished membrane obtained in an embodiment of the present invention;

[0028] Figure 2 This is a SEM image of the finished membrane obtained in an embodiment of the present invention;

[0029] Figure 3 This is a comparison chart of the capacity retention rates of the embodiments of the present invention and commercially available films. Detailed Implementation

[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0031] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0032] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0033] The finished product obtained in this invention is subjected to performance testing. The test items include water absorption rate and swelling rate, ionic conductivity and vanadium ion cross-test. The test methods are as follows:

[0034] (1) Proton conductivity:

[0035] The thickness of the sample film should be measured first before the measurement.

[0036] Fill both sides of the H-Cell with 2.5M H2SO4 solution, and measure the impedance without the film using two platinum electrodes on an electrochemical workstation (CHI760E) (open circuit voltage set to 0V, platinum electrodes placed in parallel at a distance of 9.5cm, platinum electrode size 1*1cm), with the frequency set from 100000Hz to 0.1Hz.

[0037] Then, the impedance of the sample membrane was measured three times and the average value was taken (the sample membrane was held in the middle of the H-Cell, separating the solutions on both sides of the membrane).

[0038] The proton conductivity of the membrane can be calculated using the following formula:

[0039]

[0040] Where σ is the proton conductivity of the membrane, S and d are the area and thickness of the membrane, respectively, and R is the resistance of the membrane.

[0041] (2) Vanadium ion diffusion rate:

[0042] 60 mL of 1 M VOSO4 + 2.5 M H2SO4 and 60 mL of 1 M MgSO4 + 2.5 M H2SO4 were placed on opposite sides of an H-cell, separated by a membrane. Both cells were magnetically stirred at 300 rpm / min to reduce concentration polarization.

[0043] Every hour, 3 mL of sample solution was taken from the MgSO4 side and tested using a UV spectrophotometer. Data were recorded, and a total of 10 data points were collected.

[0044] According to VO 2+ VO was calculated from the standard curve of concentration and absorbance. 2+ Concentration. VO 2+ Permeability can be calculated using the following formula:

[0045]

[0046] Where VR is the volume of the MgSO4 solution, and CR is the VO in the MgSO4 solution on the right side of the diffusion cell. 2+ The concentration of V is given by t, time is given by A, the effective area of ​​the ion exchange membrane is given by L, and V is given by P. 2+ The permeability, CL is the VO in the VOSO4 solution on the right side of the diffusion cell. 2+ The concentration.

[0047] (3) Methods for determining ion selectivity:

[0048] Ion selectivity is calculated from proton conductivity and vanadium ion selectivity, using the following formula:

[0049]

[0050] Where S is the ion selectivity, σ is the proton conductivity of the membrane, and P is the VO2max concentration. 2+ Penetration rate.

[0051] (3) Single-cell test:

[0052] The membrane to be tested was placed in the center, forming a symmetrical structure with two carbon felts and two graphite current collectors from the inside out. This was then secured with bolts to assemble the vanadium redox flow battery. The membrane dimensions were 5cm × 5cm, the carbon felt dimensions were 3cm × 3cm, and both the positive and negative electrode electrolytes were 25mL of 1mol / L VOC. 2+ / V 3+ (mol / mol = 1:1) + 25 mol L -1 A mixed solution of H2SO4. During battery operation, the charging cutoff voltage was set to 1.7V, the discharging cutoff voltage was set to 0.8V, the battery testing system was the Blue Electric charge / discharge battery testing system, and the electrolyte flow rate was 60mL / min.

[0053] Example 1

[0054] This embodiment provides a method for preparing a composite proton exchange membrane, the steps of which are as follows:

[0055] (1) Sulfonated polyether ether ketone (SPEEK) was dissolved in DMF solution and sonicated for 2 hours to obtain a homogeneous solution; wherein the ultrasonic power was 300W and the mass-volume ratio of SPEEK to DMF solution was 1g:10mL.

[0056] (2) The homogeneous solution obtained in step (1) is poured onto a clean glass plate and left to stand at room temperature for 24 hours until the membrane is set. Then the set membrane is transferred to an oven and dried at 80°C for 14 hours to obtain a SPEEK substrate membrane, wherein the thickness of the SPEEK substrate membrane is 100 micrometers.

[0057] (3) The SPEEK base membrane was completely immersed in a buffer solution (Tris-HCl buffer, pH=8.5) with magnetic stirring at a speed of 400 rpm / min. Dopamine hydrochloride (DA) was added at a rate of 1.5 g / L and the reaction was continued for 30 min to obtain a SPEEK and PDA composite membrane. The composite membrane structure consisted of two layers with a thickness ratio of 100 μm: 50 nm.

[0058] Meanwhile, the polytetrafluoroethylene (PTFE) emulsion (commercial PTFE emulsion, Zhanyang Polymer Materials, PTFE nanoparticles of 200nm, mass fraction of 60%) was diluted with buffer (Tris-HCl buffer, pH=8.5) and sonicated at 300W for 30min to disperse it evenly. The mass-volume ratio of PTFE to buffer was 0.5g:50mL.

[0059] (4) The SPEEK and PDA composite membrane obtained above was immediately and completely immersed in 100 mL of PTFE uniformly dispersed buffer solution. Under the condition of stirring speed of 400 rpm / min, 100 mL of 1.5 g / L DA was added, and the reaction was continued for 60 min. After that, it was taken out and dried in a forced-air drying oven at 40 °C for 10 h to obtain the SPEEK-based composite proton exchange membrane (the composite membrane structure is two layers with a thickness ratio of approximately 100 μm: 250 nm). For the finished membrane obtained in this example, please refer to the image. Figure 1 See the SEM image of the finished membrane. Figure 2 .

[0060] For a comparison chart of capacity retention between this embodiment and a commercially available film (Nafion 115), please refer to [link / reference needed]. Figure 3 As can be seen, the finished membrane prepared by this invention has better performance.

[0061] Example 2

[0062] This embodiment provides a method for preparing a composite proton exchange membrane, the steps of which are as follows:

[0063] (1) Sulfonated polyether ether ketone (SPEEK) was dissolved in DMF solution and sonicated for 2 hours to obtain a homogeneous solution; wherein the ultrasonic power was 300W and the mass-volume ratio of SPEEK to DMF solution was 1g:10mL.

[0064] (2) The homogeneous solution obtained in step (1) is poured onto a clean glass plate and left to stand at room temperature for 24 hours until the membrane is set. Then the set membrane is transferred to an oven and dried at 80°C for 14 hours to obtain a SPEEK substrate membrane, wherein the thickness of the SPEEK substrate membrane is 100 micrometers.

[0065] (3) The SPEEK base membrane was completely immersed in a buffer solution (Tris-HCl buffer, pH=8.5) with magnetic stirring at a speed of 400 rpm / min. Dopamine hydrochloride (DA) was added at a rate of 1.5 g / L and the reaction was continued for 30 min to obtain a SPEEK and PDA composite membrane (the composite membrane structure is two layers with a thickness ratio of approximately 100 μm: 50 nm).

[0066] Meanwhile, the polytetrafluoroethylene (PTFE) emulsion (commercial PTFE emulsion, Zhanyang Polymer Materials, PTFE nanoparticles of 200nm, mass fraction of 60%) was diluted with buffer (Tris-HCl buffer, pH=8.5) and sonicated at 300W for 30min to disperse it evenly. The mass-volume ratio of PTFE to buffer was 1.5g:50mL.

[0067] (4) The SPEEK and PDA composite membrane obtained above was immediately and completely immersed in 100 mL of PTFE uniformly dispersed buffer solution. Under the condition of stirring at 400 rpm / min, 100 mL of 1.5 g / L DA was added and the reaction was continued to obtain a SPEEK-based composite proton exchange membrane (the composite membrane structure is two layers with a thickness ratio of approximately 100 μm: 250 nm).

[0068] Example 3

[0069] This embodiment provides a method for preparing a composite proton exchange membrane, the steps of which are as follows:

[0070] (1) Sulfonated polyether ether ketone (SPEEK) was dissolved in DMF solution and sonicated for 2 hours to obtain a homogeneous solution; wherein the ultrasonic power was 300W and the mass-volume ratio of SPEEK to DMF solution was 1g:10mL.

[0071] (2) The homogeneous solution obtained in step (1) is poured onto a clean glass plate and left to stand at room temperature for 24 hours until the membrane is set. Then the set membrane is transferred to an oven and dried at 80°C for 14 hours to obtain a SPEEK substrate membrane, wherein the thickness of the SPEEK substrate membrane is 100 micrometers.

[0072] (3) The SPEEK base membrane was completely immersed in a buffer solution (Tris-HCl buffer, pH=8.5) with magnetic stirring at a speed of 400 rpm / min. Dopamine hydrochloride (DA) was added at a rate of 1.5 g / L and the reaction was continued for 30 min to obtain a SPEEK and PDA composite membrane. The composite membrane structure consisted of two layers with a thickness ratio of 100 μm: 50 nm.

[0073] Meanwhile, the polytetrafluoroethylene (PTFE) emulsion (commercial PTFE emulsion, Zhanyang Polymer Materials, PTFE nanoparticles of 200nm, mass fraction of 60%) was diluted with buffer (Tris-HCl buffer, pH=8.5) and sonicated at 300W for 30min to disperse it evenly. The mass-volume ratio of PTFE to buffer was 2.5g:50mL.

[0074] (4) The SPEEK and PDA composite membrane obtained above was immediately and completely immersed in 100 mL of PTFE uniformly dispersed buffer solution. Under the condition of stirring at 400 rpm / min, 100 mL of 1.5 g / L DA was added and the reaction was continued to obtain a SPEEK-based composite proton exchange membrane (the composite membrane structure is two layers with a thickness ratio of approximately 100 μm: 250 nm).

[0075] Comparative Example 1

[0076] (1) Sulfonated polyether ether ketone (SPEEK) was dissolved in DMF solution and sonicated for 2 hours to obtain a homogeneous solution; wherein the ultrasonic power was 300W and the mass-volume ratio of SPEEK to DMF solution was 1g:10mL.

[0077] (2) The homogeneous solution obtained in step (1) is poured onto a clean glass plate and left to stand at room temperature for 24 hours until the membrane is set. Then the set membrane is transferred to an oven and dried at 80°C for 14 hours to obtain a SPEEK substrate membrane, wherein the thickness of the SPEEK substrate membrane is 100 micrometers.

[0078] Comparative Example 2

[0079] (1) Sulfonated polyether ether ketone (SPEEK) was dissolved in DMF solution and sonicated for 2 hours to obtain a homogeneous solution; wherein the ultrasonic power was 300W and the mass-volume ratio of SPEEK to DMF solution was 1g:10mL.

[0080] (2) The homogeneous solution obtained in step (1) is poured onto a clean glass plate and left to stand at room temperature for 24 hours until the membrane is set. Then the set membrane is transferred to an oven and dried at 80°C for 14 hours to obtain a SPEEK substrate membrane, wherein the thickness of the SPEEK substrate membrane is 100 micrometers.

[0081] (3) The SPEEK base membrane was completely immersed in a buffer solution (Tris-HCl buffer, pH=8.5) with magnetic stirring at a speed of 400 rpm / min. Dopamine hydrochloride (DA) was added at a rate of 1.5 g / L and the reaction was continued for 30 min to obtain a SPEEK and PDA composite membrane. The composite membrane structure consisted of two layers with a thickness ratio of 100 μm: 50 nm.

[0082] (4) The SPEEK and PDA composite membrane obtained above was immediately and completely immersed in Tris-HCl buffer solution. Under the condition of stirring at 400 rpm / min, 100 mL of 1.5 g / L DA was added and the reaction was continued for 60 min to obtain SPEEK-based composite proton exchange membrane (the composite membrane structure is two layers with a thickness ratio of approximately 100 μm: 250 nm).

[0083] Table 1 Performance data of the finished products obtained in Examples 1-3 and the comparative examples.

[0084]

[0085]

[0086] Table 1 shows that when the PTFE content is 1%, the membrane ion selectivity is optimal, and the proton conductivity is relatively higher than that of Comparative Example 1. This is because at this time, the amino group in PDA, which acts as a PTFE linker, combines with the sulfonic acid group in SPEEK to form an acid-base pair, which promotes proton jumping. At the same time, the distribution of PTFE on the surface of SPEEK membrane inhibits the diffusion of vanadium ions.

[0087] When the mass fraction of PTFE increases, PTFE will form clusters on the surface of the SPEEK membrane, resulting in large pores and thus poor ion selectivity. When PTFE is not added, its performance deteriorates.

[0088] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the present invention.

Claims

1. A method for preparing a sulfonated polyether ether ketone-based composite proton exchange membrane, characterized in that: include, Sulfonated polyether ether ketone is added to an organic solvent and ultrasonically mixed to obtain a homogeneous solution. The organic solvent includes dimethylformamide, and the ratio of sulfonated polyether ether ketone to organic solvent is 1~4g:10~20mL. A sulfonated polyetheretherketone membrane was obtained by coating a homogeneous solution. A sulfonated polyether ether ketone (PEEEK) membrane was immersed in a buffer solution, and dopamine hydrochloride was added to prepare a composite membrane of PEEKEK and dopamine hydrochloride. The buffer solution included Tris-HCl buffer with a pH of 8.

5. The concentration of dopamine hydrochloride in the buffer solution was 1-1.5 g / L. The composite membrane had a two-layer structure, consisting of a sulfonated PEEKEK layer and a dopamine hydrochloride layer, with a thickness ratio of 80-100 μm: 20-50 nm. Polytetrafluoroethylene (PTFE) emulsion was diluted with buffer solution and ultrasonically dispersed to obtain a PTFE dispersion emulsion. The solvent was Tris-HCl buffer solution, and the mass-to-volume ratio of PTFE to buffer solution was 0.5~2.5g:20~50mL. The composite membrane of sulfonated polyether ether ketone and dopamine hydrochloride was completely immersed in a polytetrafluoroethylene dispersion emulsion. Dopamine hydrochloride was added, and the reaction was continued for 60-90 minutes. After drying, a sulfonated polyether ether ketone-based composite proton exchange membrane was obtained. The concentration of dopamine hydrochloride was 1.5 g / L, and the volume ratio of polytetrafluoroethylene dispersion emulsion to dopamine hydrochloride was 1:

1. The sulfonated polyether ether ketone-based composite proton exchange membrane had a two-layer structure with a thickness ratio of 80-100 μm: 200-250 nm.

2. The preparation method according to claim 1, characterized in that: The homogenized solution is obtained by ultrasound, wherein the ultrasound power is 200~300W.

3. The preparation method according to claim 1, characterized in that: The process of coating a homogeneous solution to obtain a sulfonated polyetheretherketone membrane includes, The homogenized solution is poured onto a clean glass plate and left to stand at room temperature for 20-24 hours until the membrane is set. The set membrane is then transferred to an oven and dried at 60-80°C for 10-14 hours to obtain a sulfonated polyether ether ketone membrane.

4. The application of the sulfonated polyether ether ketone-based composite proton exchange membrane prepared by any of the preparation methods described in claims 1 to 3 in an all-vanadium redox flow battery.

Citation Information

Patent Citations

  • Multi-layer moisture making compound film for proton exchange film fuel cell and its making method

    CN101079487A

  • Composite filling type proton exchange membrane as well as preparation method and application thereof