Method for improving single-kiln output of vanadium-nitrogen alloy prepared by pusher kiln
By adjusting the vanadium raw material ratio and optimizing the pellet density and porosity, the problem of limited nitriding rate in the high-temperature section of the pusher kiln was solved, thereby increasing the output of vanadium-nitrogen alloys in a single kiln and improving production efficiency.
Patent Information
- Application Number
- CN202311349458.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-18
AI Technical Summary
In existing technologies, how to improve the porosity of the feed balls in the high-temperature section of the pusher kiln while maintaining the output of a single kiln, especially how to increase the output of vanadium-nitrogen alloys in a single kiln, is an urgent problem to be solved.
By adjusting the proportion of vanadium raw materials, the density and porosity of the initial material balls in the high-temperature section of the pusher kiln are controlled, thereby optimizing nitriding efficiency, increasing the nitriding rate, increasing the pusher kiln speed, and achieving an increase in single-kiln output.
By adjusting the ratio of vanadium source, carbon source and binder, the density and porosity of raw pellets were optimized, significantly increasing the single-kiln output of vanadium-nitrogen alloy and improving the production efficiency of pusher kilns.
Abstract
Description
Technical Field
[0001] This invention relates to the field of vanadium metallurgy, and more particularly to a method for increasing the pushing speed of a pusher kiln in the preparation of vanadium-nitrogen alloys. Background Technology
[0002] Vanadium-nitrogen alloy is a new type of high-efficiency steel alloying additive that can play a role in grain refinement and precipitation strengthening in steel. Compared with ferrovanadium alloy, it can save 20% to 40% of vanadium usage to achieve the same strength in steel, thereby significantly reducing production costs. It can also effectively improve the comprehensive mechanical properties of steel, such as wear resistance, strength, toughness, and thermal fatigue resistance, and is widely used as a microalloying additive in the smelting of vanadium-containing steel.
[0003] Currently, the production of vanadium-nitrogen alloys mainly adopts the double-pusher kiln method. First, vanadium oxide powder is mixed evenly with graphite powder, catalyst, and binder and pressed into balls. These balls are then placed in a graphite crucible and calcined after passing through the drying section, low-temperature section, high-temperature section, and cooling section of the pusher kiln to produce a vanadium-nitrogen alloy product with a metallic luster. During production, as the raw balls move from the low-temperature section to the high-temperature section of the kiln, the graphite C in the raw balls undergoes a reduction and carbonization reaction with the vanadium oxide. At the same time, the N2 atmosphere in the kiln provides the N element required for the nitriding process of the raw balls and also plays a role in controlling the atmosphere in the kiln, reducing the oxygen partial pressure, and preventing the oxidation of the vanadium-nitrogen alloy and the graphite crucible. The carbonization and nitriding time of raw material balls in the kiln during production is mainly controlled by the reaction rate of the nitriding process. The nitriding rate of vanadium-nitrogen alloy raw material balls in the high-temperature section of the pusher kiln is closely related to the porosity of the raw material balls in the high-temperature section. Increasing the porosity of the raw material balls in the high-temperature section can significantly increase the nitriding rate of the raw material balls, but this will also reduce the density of the raw material balls, resulting in a decrease in the weight of the charge in a single crucible. How to improve the porosity of the high-temperature section while taking into account the output of a single kiln is a problem that needs to be studied.
[0004] Therefore, there is a need in the existing technology to improve the single-kiln output of pusher kilns for preparing vanadium-nitrogen alloys. Summary of the Invention
[0005] In view of this, the purpose of this invention is to propose a method for increasing the single-kiln output of vanadium-nitrogen alloys in a pusher kiln. By adjusting the proportion of vanadium raw materials to control the density and porosity of the pellets in the initial stage of the high-temperature section of the pusher kiln, the diffusion rate of N2 inside the pellets can be directly controlled, thereby improving the nitriding efficiency, directly increasing the pusher kiln speed, and increasing the single-kiln output.
[0006] To achieve the above objectives, embodiments of the present invention provide a method for increasing the single-kiln output of a pusher kiln for preparing vanadium-nitrogen alloys, comprising the following steps:
[0007] The vanadium source is ground and crushed and mixed with the carbon source and binder in a mixing equipment. The vanadium source includes at least two vanadium-containing compounds. The ratio of vanadium source, carbon source and binder by mass percentage is 10:(2-3):1, and the ratio of the two vanadium oxides in the vanadium source is (1-9):(9-1).
[0008] The mixed materials are transported to a briquetting platform for forming to obtain raw material briquettes. After aging treatment, the raw material briquettes are sent to a pusher kiln for calcination to obtain vanadium-nitrogen alloy.
[0009] In some embodiments, the ratio of the two vanadium oxides in the vanadium source is (3:7) to (7:3).
[0010] In some embodiments, the vanadium source includes V2O5, V2O3, and ammonium vanadate.
[0011] In some implementations, the mixing process includes both dry mixing and high-speed wet mixing of the materials.
[0012] In some implementations, the high-speed wet mixing rate is at least 1000 r / min.
[0013] In some embodiments, the calcination process of the raw material pellets in the pusher kiln includes: placing the raw material pellets in a graphite crucible jar, placing the jar on the conveyor rollers of the pusher kiln for pushing, and then passing through a preheating reduction section, a high-temperature section, and a cooling section before exiting the furnace to obtain a vanadium-nitrogen alloy.
[0014] In some implementations, the initial density of the raw pellets in the high-temperature section of the pusher kiln is 1.5–2.5 g / cm³. 3 .
[0015] In some embodiments, the pushing speed during calcination in a pusher kiln is 13 min / crucible to 22 min / crucible.
[0016] In some implementations, the aging process involves naturally air-drying the raw pellets at room temperature in the dark for 1 to 5 days.
[0017] In some implementations, the single-kiln output of vanadium-nitrogen alloy is 2.5 to 3.5 tons.
[0018] The present invention has at least the following beneficial technical effects:
[0019] The method of this invention controls the density of raw material pellets in the early stage of the high-temperature section of the pusher kiln and the porosity during the nitriding reaction in the high-temperature section of the pusher kiln by adjusting the batching and forming process of the raw material pellets. This directly controls the diffusion rate of N2 inside the pellets, improves the nitriding efficiency, and ultimately directly increases the pusher kiln speed and increases the output of a single kiln. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples.
[0021] The terms "comprising" and "having," and any variations thereof, in the specification and claims of this invention are intended to cover non-exclusive inclusion; the terms "first," "second," etc., in the specification and claims of this invention are used to distinguish different objects, not to describe a particular order. "A plurality of" means two or more, unless otherwise explicitly specified.
[0022] Furthermore, the reference to "embodiment" herein means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0023] Traditionally, a single vanadium source, such as V2O5 or V2O3, is used as a raw material to produce vanadium-nitrogen alloys.
[0024] The vanadium-nitrogen alloy raw material pellets prepared using V₂O₃ as the vanadium source have a high density, reaching 3.2–3.4 g / cm³. 3 Furthermore, before the pellets enter the high-temperature section of the pusher kiln, only the carburizing reaction occurs but not the reduction reaction. The pellets maintain high density and low porosity. Therefore, the diffusion rate of N2 in the pellets is low. The pellets need to stay in the high-temperature section of the pusher kiln for a sufficient period of time to maintain the chemical composition of the product. The maximum pushing speed is 22 min / crucible, and the output of a single kiln is 2.4 t / d. Therefore, the diffusion rate of N2 is the limiting factor for the output of a single kiln.
[0025] The vanadium-nitrogen alloy raw material pellets prepared using V₂O₅ as the vanadium source have a low density, ranging from 2.4 to 2.6 g / cm³. 3 Furthermore, before the pellets enter the high-temperature section of the pusher kiln, both carburizing and reduction reactions occur simultaneously, reducing the pellet density to 1.5 g / cm³. 3 Furthermore, the porosity is very high, so the nitriding reaction of the pellets is no longer limited by the diffusion rate of N2. The residence time of the pellets in the high-temperature section of the pusher kiln can be greatly shortened, and the maximum pushing speed can reach 13 min / crucible. The output of a single kiln is 2.6 t / d. At this time, the pellet density is the limiting factor for the output of a single kiln.
[0026] The carbonization and nitriding time of raw material balls in the kiln during production is mainly controlled by the reaction rate of the nitriding process. Studies have shown that the nitriding rate of vanadium-nitrogen alloy raw material balls in the high-temperature section of the pusher kiln is closely related to the porosity of the raw material balls in the high-temperature section. Increasing the porosity of the raw material balls in the high-temperature section can significantly increase the nitriding rate of the raw material balls, but this will also reduce the density of the raw material balls, resulting in a decrease in the weight of the charge in a single crucible. The output of a single kiln is a function of the pushing speed and the porosity, and there is a maximum value.
[0027] Therefore, this invention controls the porosity of the raw material pellets during the nitriding reaction in the high-temperature section of the pusher kiln by adjusting the batching and forming process. This coordinates the functional relationship between the pusher kiln speed and the output of a single kiln, obtaining the optimization direction of the independent variables of pellet porosity and pusher speed, thereby maximizing the output. The method of this invention specifically includes the following steps:
[0028] S1. Grind and crush the vanadium source and mix it with the carbon source and binder in a mixing equipment. The vanadium source includes at least two vanadium-containing compounds. By mass percentage, the ratio of vanadium source, carbon source and binder is 10:(2~3):1, and the ratio of the two vanadium oxides in the vanadium source is (1~9):(9~1).
[0029] S2. The mixed materials are transported to the briquetting platform for molding to obtain raw material briquettes. After aging treatment, the raw material briquettes are sent to the pusher kiln for calcination to obtain vanadium-nitrogen alloy.
[0030] Furthermore, in S1, the vanadium source includes V2O5, V2O3, and ammonium vanadate, etc. In some embodiments, V2O5 and V2O3 are selected, and the ratio of the two vanadium oxides by mass percentage is (3:7) to (7:3). Preferably, the ratio of V2O5 to V2O3 is 3:7. During mixing, dry mixing and high-speed wet mixing are performed separately. In some embodiments, the high-speed wet mixing rate is at least 1000 r / min.
[0031] Furthermore, in S2, the calcination process of the raw pellets in the pusher kiln includes: placing the raw pellets in a graphite crucible jar, placing the jar on the conveyor rollers of the pusher kiln for pushing, and then exiting the furnace after passing through a preheating reduction section, a high-temperature section, and a cooling section to obtain a vanadium-nitrogen alloy. The initial density of the raw pellets in the high-temperature section of the pusher kiln is 1.5–2.5 g / cm³. 3 The pushing speed during calcination in the pusher kiln is 13 min / crucible to 22 min / crucible.
[0032] Furthermore, the aging process involves naturally air-drying the raw material balls at room temperature in the dark for 1 to 5 days.
[0033] Furthermore, the single-kiln output of vanadium-nitrogen alloy is 2.5 to 3.5 tons.
[0034] The present invention will be further explained below through specific embodiments.
[0035] Example 1
[0036] V₂O₅, V₂O₃, C powder, and binder were mixed in a wet mixing apparatus at a ratio of 90:10:27:10 for 1.5 hours. After being air-dried for 2 days, the pellets were placed in a graphite crucible and fed into a pusher kiln for calcination. The initial density of the pellets in the high-temperature section was 1.6 g / cm³. 3 The maximum pushing speed of the pusher kiln is 13 min, and the output is 2.7 t / d.
[0037] Example 2
[0038] V₂O₅, V₂O₃, C powder, and binder were mixed in a wet mixing apparatus at a ratio of 70:30:26:10 for 1.5 hours. After being air-dried for 2 days, the pellets were placed in a graphite crucible and fed into a pusher kiln for calcination. The initial density of the pellets in the high-temperature section was 1.8 g / cm³. 3 The maximum pushing speed of the pusher kiln is 13 min, and the output is 3.1 t / d.
[0039] Example 3
[0040] V2O5, V2O3, C powder, and binder were mixed in a wet mixing device at a ratio of 50:50:25:10 for 1.5 hours. After being air-dried for 2 days, the pellets were placed in a graphite crucible and fed into a pusher kiln for calcination. The initial density of the pellets in the high-temperature section was 2 g / cm³. 3 The maximum pushing speed of the pusher kiln is 13 min, and the output is 3.5 t / d.
[0041] Example 4
[0042] V₂O₅, V₂O₃, C powder, and binder were mixed in a wet mixing apparatus at a ratio of 30:70:25:10 for 1.5 hours. After being air-dried for 2 days, the pellets were placed in a graphite crucible and fed into a pusher kiln for calcination. The initial density of the pellets in the high-temperature section was 2.2 g / cm³. 3 The maximum pushing speed of the pusher kiln is 15 min, and the output is 3.3 t / d.
[0043] Example 5
[0044] V₂O₅, V₂O₃, C powder, and binder were mixed in a wet mixing apparatus at a ratio of 10:90:24:10 for 1.5 hours. After being air-dried for 2 days, the pellets were placed in a graphite crucible and fed into a pusher kiln for calcination. The initial density of the pellets in the high-temperature section was 2.5 g / cm³. 3 The maximum pushing speed of the pusher kiln is 19 min, and the output is 3 t / d.
[0045] In the method of the present invention, the preferred ratio of V2O5:V2O3 is (3:7) to (7:3), and the most preferred mass ratio of V2O5:V2O3 is 3:7. At this time, the output of a single kiln can be increased to 3.5t / d, which is 35% and 45% higher than the output of single V2O5 and V2O3 vanadium-nitrogen alloy balls, respectively.
[0046] The above are exemplary embodiments disclosed in this invention. However, it should be noted that various changes and modifications can be made without departing from the scope of the embodiments of this invention as defined by the claims. The functions, steps, and / or actions of the methods according to the disclosed embodiments described herein do not need to be performed in any particular order. Furthermore, although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular number.
[0047] It should be understood that, as used herein, the singular form “a” is intended to include the plural form as well, unless the context clearly supports an exception. It should also be understood that, as used herein, “and / or” refers to any and all possible combinations of one or more of the associated listed items.
[0048] The embodiment numbers disclosed in the above embodiments of the present invention are for descriptive purposes only and do not represent the superiority or inferiority of the embodiments.
[0049] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of different aspects of the invention exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method for increasing the output of a single kiln in a pusher kiln for preparing vanadium-nitrogen alloys, characterized in that, include: The vanadium source is ground and crushed, and then mixed with the carbon source and binder in a mixing equipment. The vanadium source includes at least two vanadium-containing compounds. By mass percentage, the ratio of the vanadium source, carbon source and binder is 10:(2~3):1, and the ratio of the two vanadium oxides in the vanadium source is (1~9):(9~1). The mixed materials are transported to a briquetting platform for forming to obtain raw material briquettes. After aging treatment, the raw material briquettes are sent to a pusher kiln for calcination to obtain vanadium-nitrogen alloy. The calcination process of the raw material pellets in the pusher kiln includes: placing the raw material pellets in a graphite crucible jar, placing the jar on the conveyor rollers of the pusher kiln for pushing, and then passing through a preheating reduction section, a high-temperature section, and a cooling section before exiting the furnace to obtain a vanadium-nitrogen alloy. The initial density of the raw material pellets in the high-temperature section of the pusher kiln is 1.5~2.5 g / cm³. 3 The pushing speed during calcination in the pusher kiln is 13 min / crucible to 22 min / crucible. The aging treatment involves naturally drying the raw material balls under light-proof and room temperature conditions for 1 to 5 days.
2. The method for increasing the single-kiln output of vanadium-nitrogen alloy preparation in a pusher kiln according to claim 1, characterized in that, The ratio of the two vanadium oxides in the vanadium source is (3:7) to (7:3).
3. The method for increasing the single-kiln output of vanadium-nitrogen alloy preparation in a pusher kiln according to claim 1, characterized in that, The vanadium source includes V2O5, V2O3, and ammonium vanadate.
4. The method for increasing the single-kiln output of vanadium-nitrogen alloy preparation in a pusher kiln according to claim 1, characterized in that, The mixing process includes dry mixing and high-speed wet mixing of the materials.
5. The method for increasing the single-kiln output of a pusher kiln for preparing vanadium-nitrogen alloys according to claim 4, characterized in that, The high-speed wet mixing rate is at least 1000 r / min.
6. The method for increasing the single-kiln output of vanadium-nitrogen alloy preparation in a pusher kiln according to claim 1, characterized in that, The single-kiln output of the vanadium-nitrogen alloy is 2.5~3.5t.
Citation Information
Patent Citations
Preparation method of high-density vanadium-nitrogen alloy pellets
CN116397097A