Preparation method and application of a co3(po4)2-mo8p5 / nf total hydrolysis catalyst
By preparing the Co₃(PO₄)₂-Mo₈P₅/NF catalyst, and utilizing the synergistic effect of CoMo bimetallic phosphides and the foamed nickel substrate, the high cost and instability of noble metal catalysts were solved, achieving efficient full water splitting performance and stable electrocatalytic water splitting.
Patent Information
- Application Number
- CN202311670598.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-07
AI Technical Summary
Existing precious metal-based catalysts are limited in commercial application due to their high cost, scarcity, and instability in water electrolysis for hydrogen production and oxygen evolution reactions. There is a need to develop efficient, stable, and inexpensive non-precious metal catalysts to improve the energy conversion efficiency of the entire water electrolysis process.
A Co₃(PO₄)₂-Mo₈P₅/NF total hydrolysis catalyst was used. Through the synergistic effect of CoMo bimetallic phosphide, and using 3D structured nickel foam as a substrate, a nanowire composite catalyst was synthesized by hydrothermal-calcination method. The metal ion structure was adjusted to optimize the electronic structure and increase the active sites.
It achieves long-term maintenance of catalytic activity under alkaline conditions, reduces production costs, exhibits excellent full hydrolysis performance, and even outperforms precious metal catalysts. Moreover, it is simple to operate and easy to scale up.
Smart Images

Figure CN117661020B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical total hydrolysis technology, specifically to a method for preparing and applying a Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst. Background Technology
[0002] Currently, the continued consumption of fossil fuels and the resulting environmental pollution and energy crisis have drawn significant human attention, making the search for environmentally friendly and efficient new energy sources a key issue in current scientific research. Hydrogen energy, with its abundant resources, wide availability, clean and pollution-free operation, and renewability, is an important energy source for achieving energy transition. Water electrolysis for hydrogen production, as an environmentally friendly and sustainable energy conversion technology, has become a current research hotspot. Water electrolysis consists of two half-reactions: the oxygen evolution reaction (OER) and the hydrogen evolution reaction (HER). The theoretical voltage required for water electrolysis is 1.23V. However, in actual reactions, inherent energy barriers and complex reaction processes limit water splitting efficiency, often requiring higher overpotentials to overcome the inherent activation barrier. The rational use of catalysts can significantly reduce the activation energy of the reaction and accelerate the catalytic reaction. Currently, noble metal-based catalysts Pt and Ru are considered the most effective HER and OER catalysts; however, the high cost, scarcity, and instability of noble metal materials severely restrict their commercial application. Therefore, developing efficient, stable, and inexpensive non-noble metal catalysts is crucial for improving the energy conversion efficiency of total water splitting. Summary of the Invention
[0003] This invention overcomes the shortcomings of existing technologies and provides a method for preparing a Co3(PO4)2-Mo8P5 / NF all-hydrolysis catalyst. This invention utilizes the synergistic effect of CoMo bimetallic phosphides to regulate the metal ion structure, thereby enhancing the activity of the electrocatalyst in all-hydrolysis. Using 3D-structured nickel foam (NF) as a substrate, a nanowire-like composite catalyst Co3(PO4)2-Mo8P5 / NF was synthesized via a simple hydrothermal-calcination method. Results show that the synergistic effect of the bimetallic phosphides in Co3(PO4)2-Mo8P5 / NF optimizes the electronic structure, accelerates electron transfer, increases the active sites of the catalyst, and exhibits excellent all-hydrolysis performance. This invention is simple to operate, has low production costs, is easily scalable, and can maintain its microstructure and good catalytic activity for a long time under alkaline conditions, demonstrating potential industrial application value in electrocatalytic water splitting.
[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: a method for preparing a Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst, comprising the following steps:
[0005] (1) Cobalt sulfate heptahydrate, ammonium fluoride, and urea were dissolved in deionized water to form a homogeneous mixed solution. The mixed solution was transferred to a stainless steel high-pressure reactor lined with polytetrafluoroethylene (PTFE), and pretreated nickel foam was added for hydrothermal reaction. After the product cooled naturally, it was washed and dried to obtain the pre-Co / NF catalyst.
[0006] (2) The pre-Co / NF catalyst obtained in step (1) is placed in a tube furnace and calcined in air atmosphere. After cooling to room temperature, Co3O4 / NF catalyst is obtained.
[0007] (3) Dissolve sodium molybdate dihydrate in deionized water, stir magnetically until a uniform mixture is formed, transfer it to a stainless steel high-pressure reactor lined with polytetrafluoroethylene, add Co3O4 / NF catalyst, carry out hydrothermal reaction, and after the reaction is completed, wash and dry to obtain pre-CoMo / NF catalyst.
[0008] (4) The pre-CoMo / NF catalyst obtained in step (3) and sodium hypophosphite were placed in two ceramic boats respectively, and calcined in a tube furnace by passing argon gas through them. After cooling to room temperature, the Co3(PO4)2-Mo8P5 / NF catalyst was obtained.
[0009] Furthermore, the concentration of the cobalt sulfate heptahydrate solution in step (1) is 0.2 mol / L; the molar ratio of the cobalt sulfate heptahydrate, ammonium fluoride and urea is 1:2:5.
[0010] Furthermore, the pretreatment method for the nickel foam in step (1) is as follows: 2cm×3cm nickel foam is ultrasonically treated with 3mol / L HCl, ethanol and deionized water for 10min respectively.
[0011] Furthermore, the hydrothermal reaction conditions in step (1) are: 60℃, 30min
[0012] Furthermore, the calcination conditions in step (2) are as follows: heating to 250°C at a rate of 5°C / min at room temperature and holding for 4 hours.
[0013] Furthermore, in step (3), the concentration of sodium molybdate dihydrate dissolved in deionized water is 0.1 mol / L; the molar ratio of sodium molybdate dihydrate in step (3) to cobalt sulfate heptahydrate in step (1) is 1:2; the molar ratio of sodium molybdate dihydrate in step (3) to sodium hypophosphite in step (4) is 1:4.55; the hydrothermal reaction conditions in step (3) are 85℃ for 5 h.
[0014] Furthermore, the calcination conditions in step (4) are as follows: heating to 300°C at a rate of 2°C / min at room temperature and holding for 2 hours.
[0015] The present invention also provides the application of the Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst obtained by the above preparation method in total hydrolysis electrocatalysis.
[0016] In addition, this invention also provides a method for testing the catalytic performance of the Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst obtained by the above preparation method. The HER / OER test is performed using a three-electrode system in an electrochemical workstation. The Co3(PO4)2-Mo8P5 / NF catalyst is cut into 1cm × 0.5cm pieces and used as the working electrode, with Hg / HgO as the reference electrode, a carbon rod as the counter electrode, and potassium hydroxide solution as the electrolyte. Noble metal Ir / C is mixed with a naphthol solution and drop-coated onto a 1cm × 0.5cm blank nickel foam for testing. The total hydrolysis test is performed using a two-electrode system in an electrochemical workstation, with the prepared Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst used as both the anode and cathode, and tested in a potassium hydroxide electrolyte.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The catalyst prepared by this invention uses low-cost raw materials, has a short operation cycle, high repeatability, and is easy to scale up for production.
[0019] The preparation method described in this invention only requires conventional reaction equipment such as ovens, tube furnaces, and magnetic stirrers. The equipment is inexpensive, readily available, and easy to operate.
[0020] The material prepared by this invention exhibits excellent total hydrolysis catalytic performance; in HER testing, only an overpotential of 48.9 mV is required to achieve a current density of 10 mA cm⁻¹. -2 In the OER test, only an overpotential of 227.7mV is required to achieve a current density of 10mA cm⁻¹. -2 Its performance is even better than that of precious metal catalysts; in a stability test lasting up to 20 hours, the catalyst activity did not decline.
[0021] This invention fully utilizes the characteristics of transition metal phosphides in regulating electronic structure, accelerating electron transfer, and increasing the active sites of the catalyst. It also utilizes the synergistic effect of bimetals to effectively improve catalytic performance, exhibiting excellent overall hydrolysis catalytic performance. Attached Figure Description
[0022] Figure 1 The XRD pattern of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1.
[0023] Figure 2SEM images of the Co3O4 / NF and pre-CoMo / NF catalysts prepared in Example 1.
[0024] Figure 3 The image shows a SEM image of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1.
[0025] Figure 4 This is an EDX mapping diagram of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1.
[0026] Figure 5 The image shows the EDX spectrum of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1.
[0027] Figure 6 The HER linear sweep voltammetry is for the Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, pre-CoMo / NF obtained in Example 1, the MoP / NF catalyst obtained in Example 2, and the CoP / NF and Ir / C catalyst obtained in Example 3.
[0028] Figure 7 HER Tafel slope plots for Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, pre-CoMo / NF, CoP / NF and Ir / C catalysts.
[0029] Figure 8 The HER impedance curves of Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, pre-CoMo / NF, MoP / NF and CoP / NF catalysts in alkaline (1MKOH) electrolyte are shown.
[0030] Figure 9 The OER linear sweep voltammetry of the Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, and pre-CoMo / NF catalysts obtained in Example 1, and the CoP / NF and Ir / C catalysts obtained in Example 3.
[0031] Figure 10 The OER Tafel slope diagrams are for the Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, and pre-CoMo / NF catalysts obtained in Example 1, and the CoP / NF and Ir / C catalysts obtained in Example 3.
[0032] Figure 11The OER impedance test curves are for Co3(PO4)2-Mo8P5 / NF, Co3O4 / NF, and pre-CoMo / NF obtained in Example 1, and for CoP / NF and Ir / C catalysts obtained in Example 3.
[0033] Figure 12 The graph shows the total hydrolysis test curve of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1.
[0034] Figure 13 The voltage-time stability curve of the Co3(PO4)2-Mo8P5 / NF catalyst obtained in Example 1 in an alkaline (1M KOH) electrolyte is shown. Detailed Implementation
[0035] The present invention will be further described below with reference to specific embodiments.
[0036] Example 1
[0037] Nickel foam measuring 2cm × 3cm was cut and ultrasonically treated with 3mol / L HCl, ethanol, and deionized water for 10 min each, and then dried in a vacuum oven. 5 mmol of CoSO4·7H2O, 10 mmol of NH4F, and 25 mmol of CO(NH2)2 were dissolved in 25 mL of deionized water and magnetically stirred for 30 min until the solution was homogeneous. The mixture was then transferred to a PTFE-lined stainless steel autoclave, and the pretreated nickel foam was added. The mixture was hydrothermally reacted at 120℃ for 5 hours. After the reactants cooled naturally to room temperature, the samples were rinsed with deionized water and ethanol, and then dried in a vacuum oven. The resulting sample was calcined at 250℃ for 4 hours in air to obtain the Co3O4 / NF catalyst.
[0038] 2.5 mmol of Na₂MoO₄·2H₂O was dissolved in 25 mL of deionized water and magnetically stirred for 30 min at room temperature. The mixture and Co₃O₄ / NF were then transferred to a PTFE-lined stainless steel autoclave and hydrothermally reacted at 85 °C for 5 h. After natural cooling to room temperature, the mixture was rinsed alternately with deionized water and ethanol, and then dried in a vacuum oven to obtain the pre-CoMo / NF catalyst.
[0039] One piece of pre-CoMo / NF and 1g of NaH2PO2 were placed in two separate ceramic boats, with the NaH2PO2 placed upstream of a quartz tube and the pre-CoMo / NF placed downstream. The mixture was heated in an Ar atmosphere at 2℃·min. -1The temperature was rapidly increased to 300°C and maintained for 2 hours. After natural cooling to room temperature, the Co3(PO4)2-Mo8P5 / NF catalyst was obtained.
[0040] Example 2
[0041] Similar to Example 1, except that the first step of hydrothermal reaction and calcination reaction are not performed, the pretreated nickel foam and Na2MoO4·2H2O solution are subjected to hydrothermal reaction, and other synthesis conditions remain unchanged, to obtain the MoP / NF catalyst.
[0042] Example 3
[0043] Similar to Example 1, except that the second hydrothermal reaction is not performed and all other synthesis conditions remain unchanged, a CoP / NF catalyst can be obtained.
[0044] Example 4
[0045] Similar to Example 1, except that the phosphating calcination temperature was changed from 300°C to 250°C, the Co3(PO4)2-Mo8P5 / NF-1 catalyst could be synthesized. Under alkaline conditions, when the current density was 10 mA cm⁻¹ -2 At that time, the overpotential of HER was 58.3mV, and the overpotential of OER was 237.8mV.
[0046] Example 5
[0047] Similar to Example 1, except that the phosphating calcination temperature was changed from 300°C to 350°C, the Co3(PO4)2-Mo8P5 / NF-2 catalyst could be synthesized. Under alkaline conditions, when the current density was 10 mA cm⁻¹ -2 At that time, the overpotential of HER was 52.6mV, and the overpotential of OER was 243.2mV.
[0048] Example 6
[0049] Similar to Example 1, except that the phosphating calcination time was changed from 2 hours to 1.5 hours, the Co3(PO4)2-Mo8P5 / NF-3 catalyst could be synthesized. Under alkaline conditions, when the current density was 10 mA cm⁻¹ -2 At that time, the overpotential of HER was 63.6mV, and the overpotential of OER was 258.2mV.
[0050] Example 7
[0051] Similar to Example 1, except that the phosphating calcination time was changed from 2 hours to 2.5 hours, the Co3(PO4)2-Mo8P5 / NF-4 catalyst could be synthesized. Under alkaline conditions, when the current density was 10 mA cm⁻¹ -2At that time, the overpotential of HER was 50.9mV, and the overpotential of OER was 234.2mV.
[0052] In this invention, the catalysts prepared by the above method are subjected to necessary structural characterization and electrochemical performance testing. Figure 1 The X-ray diffraction (XRD) pattern of the catalyst Co3(PO4)2-Mo8P5 / NF is shown. Comparison with standard cards (13-0503 and 26-1274) shows that the diffraction peaks with 2θ values of approximately 35.6°, 38.9°, 42.7°, 47.0°, and 51.7° correspond to the (002) peaks of Co3(PO4)2 (PDF#13-0503). and The diffraction peaks with 2θ values of approximately 28.9°, 40.8°, and 44.5° correspond to the (002) crystal plane of Mo8P5 (PDF#26-1274). and The three diffraction peaks at 44.5°, 51.9° and 76.4° correspond to metallic Ni on the nickel foam substrate (PDF#04-0850), indicating the successful synthesis of the Co3(PO4)2-Mo8P5 / NF catalyst.
[0053] Figure 2 To prepare Co3O4 / NF ( Figure 2 a) and pre-CoMo / NF( Figure 2 The SEM image of b) shows that both exhibit a dandelion-like structure composed of uniformly distributed nanowires. Figure 3 The SEM image of the catalyst Co3(PO4)2-Mo8P5 / NF shows a randomly arranged clustered nanowire structure. Such a small and dense cluster structure can provide a larger specific surface area, expose more active sites, and thus improve the catalytic activity of Co3(PO4)2-Mo8P5 / NF. Figure 4 The EDX mapping diagram of the obtained Co3(PO4)2-Mo8P5 / NF shows that the material contains three elements: Co, Mo and P, and the three elements are uniformly distributed in the material. Figure 5 The EDX spectrum of the obtained Co3(PO4)2-Mo8P5 / NF material shows the content percentage of each element in the material.
[0054] The catalyst materials prepared by the above method were tested for electrocatalytic water splitting performance in a standard three-electrode electrolyzer. The HER cyclic scan range was -0.9 to -1.6 V, with a scan rate of 2 mV / s. The OER cyclic scan range was 0 to 1.0 V, with a scan rate of 2 mV / s. The total water splitting cyclic scan range was 1.2 to 2.0 V, with a scan rate of 2 mV / s. It should be noted that all potentials obtained using the Hg / HgO electrode as a reference electrode in the electrocatalytic tests were converted to reversible hydrogen electrode potentials in the performance graph.
[0055] Figure 6 HER linear sweep voltammetry plots for Co3(PO4)2-Mo8P5 / NF, pre-CoMo / NF, CoP / NF, MoP / NF, Co3O4 / NF, and Ir / C catalysts. Compared to other catalysts, at a current density of 10 mA cm⁻¹... -2 At this time, the overpotential of Co3(PO4)2-Mo8P5 / NF was only 48.9mV, exhibiting the best electrochemical performance.
[0056] Figure 7 The HER Tafel slope diagram of the catalyst shows that Co3(PO4)2-Mo8P5 / NF has the smallest Tafel slope, indicating that Co3(PO4)2-Mo8P5 / NF has the highest activity and the fastest reaction rate.
[0057] Figure 8 The HER impedance diagrams for the catalysts show that Co3(PO4)2-Mo8P5 / NF has the lowest impedance, indicating that it has the fastest electron transfer capability.
[0058] Figure 9 Linear sweep voltammetry (OER) plots for Co3(PO4)2-Mo8P5 / NF, pre-CoMo / NF, CoP / NF, Co3O4 / NF, and Ir / C catalysts are shown. Compared to other catalysts, Co3(PO4)2-Mo8P5 / NF requires only 227.7 mV overpotential to reach 10 mA cm⁻¹. -2 The current density exhibited the best electrochemical performance.
[0059] Figure 10 The OER Tafel slope diagram of the catalyst shows that Co3(PO4)2-Mo8P5 / NF has the smallest Tafel slope, indicating that Co3(PO4)2-Mo8P5 / NF has the fastest reaction kinetics.
[0060] Figure 11 The OER impedance diagram of the catalyst shows that Co3(PO4)2-Mo8P5 / NF has the lowest impedance, indicating that it has the lowest reaction resistance and the fastest electron transfer rate.
[0061] Figure 12 Linear sweep voltammogram of the Co3(PO4)2-Mo8P5 / NF catalyst for the complete hydrolysis, as a complete hydrolysis cell at a current density of 10 mA cm⁻¹ -2 At that time, the battery voltage was only 1.41V.
[0062] Figure 13 The two electrodes, Co3(PO4)2-Mo8P5 / NF and Co3(PO4)2-Mo8P5 / NF, are used at a current density of 10 mA cm⁻¹. -2 Stability test chart. As can be seen, it ran stably for 20 hours, indicating good overall hydrolysis durability.
Claims
1. A method for preparing a Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst, characterized in that, Includes the following steps: (1) Cobalt sulfate heptahydrate, ammonium fluoride, and urea were dissolved in deionized water in a molar ratio of 1:2:5 to form a homogeneous mixed solution, wherein the concentration of the cobalt sulfate heptahydrate solution was 0.2 mol / L. The mixed solution was transferred to a stainless steel high-pressure reactor lined with polytetrafluoroethylene, and pretreated nickel foam was added. The mixture was then hydrothermally reacted at 120°C for 5 hours. After the product cooled naturally, it was washed and dried to obtain the pre-Co / NF catalyst. (2) The pre-Co / NF catalyst obtained in step (1) was placed in a tube furnace and calcined in air atmosphere. The calcination conditions were: heating to 250°C at a rate of 5 °C / min at room temperature and holding for 4 h; after cooling to room temperature, Co3O4 / NF catalyst was obtained. (3) Sodium molybdate dihydrate is dissolved in deionized water and magnetically stirred until a uniform mixture is formed. Then, it is transferred to a stainless steel high-pressure reactor lined with polytetrafluoroethylene, and Co3O4 / NF catalyst is added. The mixture is hydrothermally reacted at 85°C for 5 hours. After the reaction is completed, it is washed and dried to obtain the pre-CoMo / NF catalyst. The concentration of sodium molybdate dihydrate dissolved in deionized water in step (3) is 0.1 mol / L. The molar ratio of sodium molybdate dihydrate in step (3) to cobalt sulfate heptahydrate in step (1) is 1:
2. (4) The pre-CoMo / NF catalyst obtained in step (3) and sodium hypophosphite were placed in two ceramic boats respectively, and calcined in a tube furnace by purging with argon gas. The calcination conditions were: heating to 300°C at a rate of 2°C / min at room temperature and holding for 2 hours; after cooling to room temperature, Co3(PO4)2-Mo8P5 / NF catalyst was obtained; wherein the molar ratio of sodium molybdate dihydrate in step (3) and sodium hypophosphite in step (4) was 1:4.
55.
2. The method for preparing a Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst according to claim 1, characterized in that, The pretreatment method for nickel foam in step (1) is as follows: 2 cm × 3 cm nickel foam is ultrasonically treated with 3 mol / L HCl, ethanol and deionized water for 10 min respectively.
3. The application of a Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst obtained by the preparation method as described in claim 1 or 2 in total hydrolysis electrocatalysis.
4. A method for testing the catalytic performance of the Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst obtained by the preparation method as described in claim 1 or 2, characterized in that, The HER / OER test was conducted in an electrochemical workstation using a three-electrode system. The Co3(PO4)2-Mo8P5 / NF catalyst was cut into 1 cm × 0.5 cm pieces and used as the working electrode. Hg / HgO was used as the reference electrode, a carbon rod was used as the counter electrode, and potassium hydroxide solution was used as the electrolyte. The total hydrolysis test was conducted in an electrochemical workstation using a two-electrode system, with the prepared Co3(PO4)2-Mo8P5 / NF total hydrolysis catalyst serving as both the anode and cathode, and the test was performed in a potassium hydroxide electrolyte.
Citation Information
Patent Citations
Cobalt-molybdenum alloy and cobalt-molybdenum mixed oxide electrocatalyst and preparation method and application thereof
CN113621987A
Preparation method and application of NiCuP-coated CeO2 / NF oxygen evolution electrocatalyst
CN116815239A