A device and method for pre-cracking a steel pipe for stress corrosion cracking test
By combining an internal bending device and an external bending device with a loading rod in a prefabrication method, along with potential difference monitoring technology, the problem of low prefabrication accuracy of fatigue cracks in full-size specimens has been solved, achieving higher accuracy and stability in crack propagation simulation, which is suitable for stress corrosion cracking tests.
Patent Information
- Application Number
- CN202211055918.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-31
AI Technical Summary
Existing technologies cannot accurately pre-induce fatigue cracks in full-size specimens, thus failing to simulate the actual service conditions of natural gas pipelines and affecting the accuracy of stress corrosion cracking tests.
An internal bending device and an external bending device are used in conjunction with a loading rod to precisely pre-induce fatigue cracks through a tube ring preloading method. The crack propagation is monitored in real time using a potential difference acquisition system, and the loading process is controlled by combining the load-COD opening displacement curve.
It improves the precision and ease of operation of fatigue crack pre-fabrication, ensures the stability and accuracy of crack propagation, and can better simulate the real service conditions of natural gas pipelines.
Smart Images

Figure CN117664670B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of stress corrosion technology for natural gas pipelines, specifically relating to a device and method for pre-fabricating fatigue cracks in steel pipes for stress corrosion cracking tests. Background Technology
[0002] Stress corrosion cracking is one of the main forms of corrosion damage in buried natural gas pipelines. Natural gas pipelines are prone to stress corrosion cracking accidents under buried soil environments, cathodic protection environments, and complex loads. Numerous cases of stress corrosion cracking failures have been documented internationally. Because leaks and explosions following stress corrosion cracking failures in natural gas pipelines often lead to catastrophic consequences, extensive research on stress corrosion cracking has been conducted in various countries.
[0003] Studies on stress corrosion cracking typically employ standard or full-size specimens under electrochemical environments and load conditions, focusing on crack propagation in pre-existing standard or full-size specimens under simulated service environments and loads. Currently, fatigue cracks can be pre-existed in standard specimens according to relevant testing standards. However, full-size tests struggle to pre-exist fatigue cracks due to the difficulty in applying fatigue loads at specified locations. Defects are usually pre-existing using electrical discharge machining or blade extrusion, with a defect tip width of approximately 0.3 mm. This defect exhibits a significant difference in stress distribution at the crack tip compared to actual cracks formed during pipeline service, making it difficult to simulate real service conditions and affecting the accuracy of stress corrosion cracking tests on full-size specimens. Summary of the Invention
[0004] The purpose of this invention is to provide a device and method for pre-fabricating fatigue cracks in steel pipes for stress corrosion cracking testing, so as to solve the technical problem that the existing pre-fabricated fatigue cracks have low accuracy and cannot simulate real service conditions.
[0005] In a first aspect, a fatigue crack pre-fabrication device for steel pipes used in stress corrosion cracking tests includes a test piece, a support device, a loading rod, an inner bending device, and an outer bending device. The test piece has a pre-fabricated defect on its surface. A COD gauge and a potential difference acquisition system are located on both sides of the pre-fabricated defect. The midpoints of the outer bending device and the inner bending device are aligned with the pre-fabricated defect. The outer bending device is located on the outside of the test piece, and the inner bending device is located on the inside of the test steel pipe. The support device is located inside the test steel pipe to support the inner bending device. A loading rod is located above the outer bending device, and the loading rod is used to apply pressure to the outer bending device.
[0006] A further improvement of the present invention is that it also includes a height adjustment device, which is disposed between the inner bending device and the support device.
[0007] A further improvement of the present invention is that: the inner bending device includes a first base and a first fixing rod; the bottom of the first base is connected to the support device, and two first fixing rods are symmetrically arranged above the first base;
[0008] The external bending device includes a second base and a second fixing rod. The second base is fixedly connected to the loading rod above it, and two second fixing rods are symmetrically arranged below the second base.
[0009] A further improvement of the present invention is that the potential difference acquisition system includes current probes symmetrically arranged on both sides of the prefabricated defect and voltage probes symmetrically arranged on both sides of the prefabricated defect.
[0010] A further improvement of the present invention is that the loading capacity of the loading rod is greater than or equal to 250kN.
[0011] A further improvement of the present invention is that the test piece includes a test steel pipe or a pipe ring.
[0012] Secondly, a method for pre-inducing fatigue cracks in steel pipes for stress corrosion cracking testing includes the following steps:
[0013] Fix the tube ring between the inner bending device and the outer bending device, so that the prefabricated defects on the tube ring are aligned with the center of the inner bending device and the outer bending device.
[0014] The loading rod applies a load, and the load-COD opening displacement curve is generated using the COD gauge.
[0015] The maximum load is obtained from the load-COD open displacement curve;
[0016] Remove the tube ring, replace it with the test steel pipe, and apply fatigue load to the loading rod according to the maximum load to pre-induce cracks;
[0017] During the pre-crack process, the change in potential difference on both sides of the pre-crack is monitored by a potential difference acquisition system, and the crack depth is calculated based on the change in potential difference on both sides of the pre-crack.
[0018] When the crack depth reaches the preset crack size, the loading rod stops loading, resulting in a stress corrosion test steel pipe with fatigue cracks of the specified size.
[0019] A further improvement of the present invention is that the fatigue load is 30% to 60% nF, where n is a constant, and the fatigue load stress ratio is 0.1 to 0.9.
[0020] A further improvement of the present invention is that the value of n ranges from 1.2 to 1.5.
[0021] A further improvement of the present invention is that: when obtaining the maximum load based on the load-COD open displacement curve, the specific steps include:
[0022] When the load in the load-COD open displacement curve drops to the preset load, stop loading and record the maximum load F corresponding to the linear segment in the load-COD open displacement curve.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects:
[0024] 1. This invention uses an internal bending device and an external bending device to bend and pre-induce fatigue cracks in test steel pipes or pipe rings. Compared with conventional EDM or blade machining, it has higher precision and is more convenient to operate.
[0025] 2. This invention uses a pipe ring preloading method to determine a reasonable fatigue load for the test steel pipe, avoiding the problem of cracks not propagating due to excessively small fatigue loads or cracks becoming unstable due to excessively large fatigue loads, thereby improving stability;
[0026] 3. This invention uses the potential difference method to monitor crack propagation in real time to obtain fatigue cracks of a specified size, making the generated fatigue cracks more accurate. Attached Figure Description
[0027] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0028] In the attached diagram:
[0029] Figure 1 This is a schematic diagram of the structure of a steel pipe fatigue crack pre-fabrication device for stress corrosion cracking test according to the present invention;
[0030] Figure 2 This is a schematic diagram of the COD gauge structure in a steel pipe fatigue crack pre-fabrication device for stress corrosion cracking testing according to the present invention.
[0031] Figure 3 This is a schematic diagram of the potential difference acquisition system in a steel pipe fatigue crack pre-fabrication device for stress corrosion cracking test according to the present invention.
[0032] Figure 4 This invention relates to a load-COD displacement curve in a method for pre-fabricating fatigue cracks in steel pipes used in stress corrosion cracking tests.
[0033] In the figure, 1. Loading rod; 2. Inner bending device; 21. First base; 22. First fixing rod; 3. Prefabricated defect; 4. Test steel pipe; 5. Height adjustment device; 6. Support device; 7. Fixing device; 8. Outer bending device; 81. Second base; 82. Second fixing rod; 9. COD gauge; 10. Current probe; 11. Voltage probe. Detailed Implementation
[0034] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other.
[0035] The following detailed description is exemplary and intended to provide further detailed explanation of the invention. Unless otherwise specified, all technical terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. The terminology used in this invention is for describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention.
[0036] Example 1
[0037] A fatigue crack pre-fabrication device for steel pipes used in stress corrosion cracking tests, such as Figure 1 As shown, the system includes a test steel pipe 4, a fixing device 7, a support device 6, a height adjustment device 5, a pre-fabricated defect 3, an inner bending device 2, an outer bending device 8, and a loading rod 1. The fixing device 7 consists of two triangular blocks with their hypotenuses facing each other. The test steel pipe 4 is positioned in the middle of the fixing device 7. The surface of the test steel pipe 4 has a pre-fabricated defect 3. Rotating the test steel pipe 4 causes the pre-fabricated defect 3 to be located at the top of the test steel pipe 4. The support device 6 is located below the inner wall of the test steel pipe 4. The bottom surface of the support device 6 is arc-shaped, and the arc is the same as the arc of the inner wall of the test steel pipe 4. The height adjustment device 5 is located above the support device 6, and the inner bending device 2 is located above the height adjustment device 5. The height adjustment device 5 is an electric telescopic rod, which adjusts the height of the inner bending device 2 and is suitable for test steel pipes 4 with different inner diameters. The inner bending device 2 includes a first base 21 and a first fixing rod 22. The first base 21 is positioned above the height adjustment device 5, and its center is aligned with the pre-fabricated defect 3. Two first fixing rods 22 are symmetrically arranged above the first base 21, and both first fixing rods 22 are in contact with the inner wall of the test steel pipe 4. An outer bending device 8 is provided on the outer side of the top of the test steel pipe 4. The outer bending device 8 includes a second base 81 and a second fixing rod 82. The center of the second base 81 is aligned with the pre-fabricated defect 3, and two second fixing rods 82 are symmetrically arranged on the lower surface of the second base 81. Both second fixing rods 82 are in contact with the outer wall of the test steel pipe 4, and the distance between the two second fixing rods 82 is not equal to the distance between the two first fixing rods 22. A loading rod 1 is provided above the second base 81, and the loading rod 1 is used to apply a vertical force to the outer bending device 8. The test piece includes a test steel pipe (4) or a pipe ring.
[0038] like Figure 2 As shown, the surface of prefabricated defect 3 is equipped with a COD gauge 9. (As indicated...) Figure 3As shown, a potential difference acquisition system is provided on both sides of the prefabricated defect 3. The potential difference acquisition system includes a current probe 10 and a voltage probe 11. Two current probes 10 are symmetrically arranged on both sides of the prefabricated defect 3, and two voltage probes 11 are also arranged on both sides of the prefabricated defect 3. The current probes 10 are used to apply a constant current to the plane where the prefabricated defect 3 is located, and the voltage probes 11 are used to detect the potential difference on both sides of the prefabricated defect 3.
[0039] As a preferred embodiment, the distance between the two current probes 10 is D / 8, where D is the diameter of the test piece.
[0040] As a preferred embodiment, the distance between the two voltage probes 11 is 5mm.
[0041] As a preferred embodiment, an electric spark or a cutting tool is used to process longitudinal pre-fabricated defects 3 with a length L and a depth a0 on the inner or outer wall of the test steel pipe 4 and the pipe ring, respectively.
[0042] As a preferred embodiment, the loading capacity of the loading rod 1 is greater than or equal to 250kN.
[0043] As a preferred embodiment, both the current probe 10 and the voltage probe 11 are fixed to both sides of the prefabricated defect 3 by welding.
[0044] Example 2
[0045] A method for pre-fabricating fatigue cracks in steel pipes for stress corrosion cracking tests, such as... Figure 4 As shown, it includes the following steps:
[0046] S1. Fix the pipe ring between the inner bending device 2 and the outer bending device 8, so that the prefabricated defect 3 on the pipe ring is aligned with the center of the inner bending device 2 and the outer bending device 8.
[0047] S2. The loading rod 1 applies an axial compressive load and generates a load-COD opening displacement curve through the COD gauge 9 set on the surface of the prefabricated defect 3. When the load in the load-COD opening displacement curve drops to the preset load, the loading is stopped, and the maximum load F corresponding to the linear segment in the load-COD opening displacement curve is recorded.
[0048] In a preferred embodiment, the preset load is 90% of the maximum load.
[0049] S3. Remove the tube ring and replace it with the test steel pipe 4. Apply fatigue load to the loading rod 1 to pre-crack.
[0050] In a preferred embodiment, the fatigue load is 30% to 60% nF.
[0051] In a preferred embodiment, n is a constant, with a value ranging from 1.2 to 1.5; the fatigue load stress ratio ranges from 0.1 to 0.9.
[0052] S4. During the pre-crack process, the change of potential difference on both sides of the pre-crack is monitored by the potential difference acquisition system, and the crack depth is calculated based on the change of potential difference on both sides of the pre-defect 3.
[0053] a=a1+a2*U+a3*U 2 +a4*U 3 ;
[0054] In the formula, a is the crack depth; a1 is the initial crack depth, which is equal to a0; U is the dimensionless potential difference, U=E / E0-1, where E is the measured DC potential difference; E0 is the potential difference corresponding to the initial crack; a2=9.55; a3=-5.21; a4=1.89;
[0055] S5. When the crack depth a reaches the preset crack size, stop the fatigue loading to obtain a stress corrosion test steel pipe containing fatigue cracks of the specified size.
[0056] Example 3
[0057] A method for pre-fabricating fatigue cracks in steel pipes for stress corrosion cracking tests includes the following steps:
[0058] 1) Prepare OD426mm*7mmX52 steel pipes and pipe rings of the same specifications for stress corrosion cracking tests. The test steel pipe is 4000mm long and the pipe ring is 500mm long.
[0059] 2) Longitudinal defects with a length of 100 mm and a depth of 4 mm were machined on the outer wall of the test steel pipe and pipe ring respectively by electrical discharge machining.
[0060] 3) Install COD gauge 9 on the surface of precast defects in the pipe ring, such as... Figure 2 As shown, the tube ring is installed Figure 1 On the apparatus shown, the testing machine applies an axial compressive load and records the load-COD opening displacement curve, as follows. Figure 4 As shown. When the load drops to 90% of the maximum load, stop loading and remove the pipe ring. Take the linear segment of the load-COD open displacement curve corresponding to the maximum load of 135kN.
[0061] 4) The test steel pipe is installed on the fatigue crack pre-fabrication device. The testing machine applies a fatigue load to pre-fabricate the crack. The maximum fatigue load is taken as 60%·nF = 105kN, where n is taken as 1.3 and the stress ratio is taken as 0.5. Current contacts and voltage contacts are welded to both sides of the pre-fabricated defect in the test steel pipe, respectively. A constant current is applied, and the voltage change on both sides of the crack is monitored. Figure 3 As shown, the initial defect corresponds to a potential difference of 29V.
[0062] 5) Apply fatigue load to the test steel pipe and monitor the change in potential difference on both sides of the crack during the pre-fatigue cracking process.
[0063] From a=a1+a2*U+a3*U 2 +a4*U 3 ;
[0064] In the formula, a is the crack depth; a1 is the initial crack depth, which is equal to a0; U is the dimensionless potential difference, U=E / E0-1, where E is the measured DC potential difference; E0 is the potential difference corresponding to the initial crack; a2=9.55; a3=-5.21; a4=1.89;
[0065] When the potential difference reaches 32V, the corresponding crack propagation is 1mm, which meets the requirements of the full-size stress corrosion cracking test.
[0066] Prepare a pipe ring with the same specifications as the test steel pipe 4, but shorter in length. The prefabrication defect size of the pipe ring is the same as that of the test steel pipe.
[0067] As is known from common technical knowledge, this invention can be implemented through other embodiments that do not depart from its spirit or essential characteristics. Therefore, the disclosed embodiments described above are merely illustrative in all respects and are not the only ones. All modifications within the scope of this invention or equivalent to the scope of this invention are included in this invention.
[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A fatigue crack pre-fabrication device for steel pipes used in stress corrosion cracking tests, characterized in that, It includes a fixing device (7), a support device (6), a height adjustment device (5), a loading rod (1), an inner bending device (2), an outer bending device (8), a COD gauge (9), and a potential difference acquisition system; The fixing device (7) includes two triangular blocks with their hypotenuses facing each other, which are used to replaceably fix the pipe ring and the test steel pipe (4) of the same specification as the pipe ring. Both the pipe ring and the test steel pipe (4) are provided with longitudinal prefabricated defects (3), and the size of the prefabricated defect (3) of the pipe ring is the same as the size of the prefabricated defect (3) of the test steel pipe (4). When the test steel pipe (4) is fixed in the fixing device (7), the prefabricated defect (3) is located at the top of the test steel pipe (4), the support device (6) is set inside the test steel pipe (4) and the bottom surface of the support device (6) is an arc with the same curvature as the inner wall of the test steel pipe (4). The height adjustment device (5) is set between the support device (6) and the inner bending device (2) to adjust the height of the inner bending device (2). The inner bending device (2) is set inside the test steel pipe (4), and the outer bending device (8) is set outside the test steel pipe (4). The centers of the inner bending device (2) and the outer bending device (8) are aligned with the prefabricated defect (3). A loading rod (1) is provided above the outer bending device (8). The COD gauge (9) is set on the surface of the prefabricated defect (3) of the pipe ring to generate a load-COD opening displacement curve when the pipe ring is subjected to an axial compressive load applied by the loading rod (1), and the maximum load F is determined by the linear segment of the load-COD opening displacement curve. The loading rod (1) is also used to apply fatigue load to the test steel pipe (4) according to the maximum load F after the pipe ring is removed and the test steel pipe (4) is replaced to pre-crack; The potential difference acquisition system is set on both sides of the prefabricated defect (3) of the test steel pipe (4) to monitor the change of potential difference on both sides of the prefabricated defect (3) during the prefabrication process, and to calculate the crack depth according to the following formula: a = a1 + a2*U + a3*U 2 + a4*U 3 ; In the formula, a is the crack depth, a1 is the initial crack depth, U is the dimensionless potential difference and U=E / E0-1, E is the measured DC potential difference, E0 is the potential difference corresponding to the initial crack, a2=9.55; a3=-5.21; a4=1.89; when the crack depth reaches the preset crack size, the loading rod (1) stops loading.
2. The apparatus according to claim 1, wherein The height adjustment device (5) is an electric telescopic rod. The height of the inner bending device (2) is adjusted by the height adjustment device (5) to adapt to test steel pipes (4) with different inner diameters.
3. The apparatus according to claim 1, wherein The internal bending device (2) includes a first base (21) and two first fixing rods (22). The first base (21) is set above the height adjustment device (5). The center of the first base (21) is aligned with the prefabricated defect (3). The two first fixing rods (22) are symmetrically set above the first base (21) and both are in contact with the inner wall of the test steel pipe (4). The external bending device (8) includes a second base (81) and two second fixing rods (82). The center of the second base (81) is aligned with the prefabricated defect (3). The two second fixing rods (82) are symmetrically arranged below the second base (81) and both are in contact with the outer wall of the test steel pipe (4). The distance between the two second fixing rods (82) is not equal to the distance between the two first fixing rods (22).
4. The apparatus according to claim 1, wherein The potential difference acquisition system includes two current probes (10) and two voltage probes (11). The two current probes (10) are symmetrically arranged on both sides of the prefabricated defect (3) and are used to apply a constant current to the plane where the prefabricated defect (3) is located. The two voltage probes (11) are arranged on both sides of the prefabricated defect (3) and are used to detect the potential difference on both sides of the prefabricated defect (3). The distance between the two current probes (10) is D / 8, where D is the diameter of the test piece, and the distance between the two voltage probes (11) is 5mm.
5. The apparatus according to claim 1, wherein The loading capacity of the loading rod (1) is greater than or equal to 250kN.
6. The apparatus according to claim 1, wherein Prefabricated defects (3) are longitudinal prefabricated defects of length L and depth a0 that are processed on the inner or outer wall of the test steel pipe (4) and the pipe ring by electric spark or blade respectively.
7. A method of preparing a fatigue crack in a steel pipe for a stress corrosion cracking test, characterized by, The fatigue crack pre-fabrication device for steel pipes used in stress corrosion cracking tests according to any one of claims 1 to 6 includes the following steps: Prepare a test steel pipe and a pipe ring of the same specifications but shorter in length. Machin the same longitudinal pre-fabricated defects on the test steel pipe and the pipe ring respectively. Fix the tube ring between the inner bending device (2) and the outer bending device (8) so that the prefabricated defect (3) on the tube ring is aligned with the center of the inner bending device (2) and the outer bending device (8); The loading rod (1) applies an axial compressive load and generates a load-COD opening displacement curve through the COD gauge (9). When the load in the load-COD opening displacement curve drops to the preset load, the loading is stopped and the maximum load F corresponding to the linear segment in the load-COD opening displacement curve is recorded. Remove the tube ring and replace it with the test steel pipe (4). Apply fatigue load to the loading rod (1) according to the maximum load F to pre-crack; During the pre-crack process, the change in potential difference on both sides of the pre-crack defect (3) is monitored by a potential difference acquisition system, and the crack depth is calculated according to the following formula: a=a1+a2×U+a3×U^2+a4×U^3; In the formula, a is the crack depth, a1 is the initial crack depth and equal to a0, U is the dimensionless potential difference and U=E / E0-1, E is the measured DC potential difference, E0 is the potential difference corresponding to the initial crack, a2=9.55, a3=-5.21, a4=1.89; When the crack depth reaches the preset crack size, fatigue loading is stopped, and a stress corrosion test steel pipe containing fatigue cracks of the specified size is obtained.
8. The method of claim 7, wherein the steel pipe is a steel pipe for stress corrosion cracking test. The fatigue load is 30% to 60% nF, where n is a constant and its value ranges from 1.2 to 1.
5. The fatigue load stress ratio is 0.1 to 0.
9.
9. The method of claim 7, wherein the steel pipe is a steel pipe for stress corrosion cracking test. The preset load is 90% of the maximum load.
10. The method of claim 7, wherein the steel pipe is a steel pipe for stress corrosion cracking test. The prefabricated defect (3) is processed by electric spark, and current contact and voltage contact are welded on both sides of the prefabricated defect (3), constant current is applied, and voltage change on both sides of the prefabricated defect (3) is monitored.
Citation Information
Patent Citations
Axial surface type crack steel pipe bursting test device and fracture resistance evaluation method thereof
CN112393969A
Bending fixture used for prefabricating fatigue crack
CN201497676U