Optical solar reflector and method of making same
By forming a high-emissivity emission layer and a multi-layer structure on the emission base surface of the optical solar reflector, the problem of insufficient heat dissipation performance is solved, achieving higher heat dissipation performance and resistance to ultraviolet radiation, thereby improving the space adaptability and lifespan of the spacecraft.
Patent Information
- Application Number
- CN202211059888.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-31
AI Technical Summary
Existing optical solar reflectors have low heat dissipation performance and cannot meet the heat dissipation requirements of high-power and long-life equipment in communication satellites.
One or more emission sublayers are formed on one side surface of the emission base layer. The emissivity of the emission layer is higher than that of the emission base layer. Combined with an ultraviolet reflection layer, a transparent conductive film and a metal reflection layer, a multi-layer structure is formed to improve heat dissipation performance and resistance to ultraviolet radiation.
It improves the heat dissipation performance and UV radiation resistance of optical solar reflectors, enhances the spacecraft's adaptability to the space environment, and extends its service life.
Smart Images

Figure CN117665991B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal control thin film technology for spacecraft, specifically to an optical solar reflector and its preparation method. Background Technology
[0002] The thermal control system is an important subsystem of a spacecraft. Because the spacecraft operates in an extremely high vacuum environment, the gas around the spacecraft is extremely thin, and the heat exchange between the spacecraft and the external environment is almost entirely carried out by radiation. In order to ensure the normal operation of the spacecraft and its internal instruments and equipment, it is necessary to use technical means to keep the spacecraft within a suitable temperature range.
[0003] An optical solar reflector, also known as a secondary surface mirror, has one surface with a high emissivity film and the other surface with a metallic film. Optical solar reflectors are characterized by low absorptivity and high emissivity, making them one of the thermal control products with the lowest absorptivity-emissivity ratio currently available.
[0004] As communication satellites develop towards higher power and longer lifespan, and as the number of instruments and equipment on spacecraft increases, the requirements for heat dissipation and / or adaptability to the space environment for these instruments and equipment also increase. Therefore, higher requirements are placed on the heat dissipation performance and / or space environment adaptability of optical solar reflectors. Summary of the Invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect of low heat dissipation performance of optical solar reflectors in the prior art, thereby providing an optical solar reflector and its manufacturing method.
[0006] The present invention provides an optical solar reflector, comprising: a reflective substrate; and a reflective layer located on one side surface of the reflective substrate, wherein the emissivity of the reflective layer is greater than that of the reflective substrate.
[0007] Optionally, the emission layer may include one or more stacked emission sublayers.
[0008] Optionally, the emitter sublayer may include an oxide emitter sublayer.
[0009] Optionally, the material of the oxide emitter layer includes one or more of silicon dioxide, titanium dioxide, aluminum oxide, and nickel oxide.
[0010] Optionally, the thickness of the emitting layer is 100nm~2000nm.
[0011] Optionally, the emission layer is composed of clustered particles.
[0012] Optionally, it may also include: an ultraviolet reflective layer located on the surface of the emitting layer opposite to the emitting substrate, the ultraviolet reflective layer comprising one or more stacked ultraviolet reflective sublayers.
[0013] Optionally, the material of the ultraviolet reflective sublayer includes an oxide ultraviolet reflective sublayer.
[0014] Optionally, the material of the oxide ultraviolet reflective sublayer includes one or a combination of titanium dioxide, cerium oxide, or zinc oxide.
[0015] Optionally, the thickness of the ultraviolet reflective layer is 50nm~300nm.
[0016] Optionally, it may also include a transparent conductive film located on the surface of the ultraviolet reflective layer facing away from the emitting layer.
[0017] Optionally, the thickness of the transparent conductive film is 5nm to 50nm.
[0018] Optionally, it may also include: a metal reflective layer located on the surface of the emitting substrate facing away from the emitting layer; the optical solar reflector may also include: a metal protective layer located on the surface of the metal reflective layer facing away from the emitting substrate.
[0019] Optionally, the material of the metal reflective layer includes silver, aluminum, copper, bismuth, germanium, or chromium.
[0020] Optionally, the material of the metal protective layer includes a nickel-based alloy.
[0021] Optionally, the base layer may include a flexible base layer or a rigid base layer.
[0022] Optionally, the thickness of the flexible base layer is 1μm to 150μm.
[0023] Optionally, the thickness of the rigid base layer is 0.05mm to 0.2mm.
[0024] Optionally, the material of the flexible base layer includes perfluoroethylene propylene or polyimide.
[0025] Optionally, the material of the rigid base layer includes quartz glass or cerium-doped glass.
[0026] The present invention also provides a method for manufacturing an optical solar reflector, comprising: providing an emitting substrate; forming an emitting layer on one side surface of the emitting substrate, wherein the emissivity of the emitting layer is greater than the emissivity of the emitting substrate.
[0027] Optionally, the method of forming an emission layer on one side surface of the emission substrate includes: forming one or more stacked emission sub-layers on one side surface of the emission substrate; the stacked emission sub-layers include a first emission sub-layer to an Nth emission sub-layer stacked sequentially, the first emission sub-layer being located between the Nth emission sub-layer and the emission substrate; N is an integer greater than or equal to 2.
[0028] Optionally, the step of forming the nth emitter sublayer includes: forming an emitter layer sol solution using a sol-gel method; applying the emitter layer sol solution to one side surface of the emitter substrate for the nth time; and performing a curing treatment on the emitter layer sol solution on the emitter substrate for the nth time to form the nth emitter sublayer; where n is an integer greater than or equal to 1 and less than or equal to N.
[0029] Optionally, the process of coating the emissive layer sol onto one side surface of the emissive substrate includes dip coating, roll coating, or spin coating.
[0030] Optionally, the parameters of the immersion-lifting method include: an immersion speed of 3000 μm / s to 5000 μm / s in the emissive layer sol, a lifting speed of 1000 μm / s to 2000 μm / s, and an immersion time of 1 min to 3 min in the emissive layer sol.
[0031] Optionally, the temperature of the first curing treatment to the temperature of the (N-1)th curing treatment is less than the temperature of the Nth curing treatment; the time of the first curing treatment to the time of the (N-1)th curing treatment is less than the time of the Nth curing treatment.
[0032] Optionally, the temperature difference between the Nth curing treatment and the kth curing treatment is 50℃~200℃; the time difference between the Nth curing treatment and the kth curing treatment is 30min~50min; k is an integer greater than or equal to 1 and less than or equal to N-1.
[0033] Optionally, during the formation of the k-th emitter layer, the temperature of the k-th curing treatment is 200℃~300℃, and the time of the k-th curing treatment is 20min~30min.
[0034] Optionally, during the formation of the Nth emitter layer, the temperature of the Nth curing treatment is 200℃~500℃, and the time of the Nth curing treatment is 50min~80min.
[0035] Optionally, the emitter sol includes one or a combination of silica sol, titanium sol, aluminum sol, zirconium sol, or nickel sol.
[0036] Optionally, the steps of forming the emission layer sol using the sol-gel method include: providing a first raw material and an alcohol, an acid solution, and a surfactant; dissolving the surfactant in the alcohol and stirring uniformly; after dissolving the surfactant in the alcohol and stirring uniformly, adding the acid solution and the first raw material and stirring; and after adding the acid solution and the first raw material and stirring, aging the mixture to form the emission layer sol.
[0037] Optionally, in the step of adding the acid solution and the first raw material and stirring, the stirring time is 6h~24h.
[0038] Optionally, the aging process can be carried out for 7 to 30 days.
[0039] Optionally, the molar ratio of the first raw material to the alcohol is 1:18 to 1:25; the molar ratio of the alcohol to the acid solution is 0.1 to 25: 0.2 to 25; and the molar ratio of the acid solution to water is 0.2: 8 to 0.2: 12.
[0040] Optionally, the acid solution includes: hydrochloric acid solution, nitric acid solution, or acetic acid solution.
[0041] Optionally, the molar concentration of the acid solution is 0.12 mol / L to 0.18 mol / L.
[0042] Optionally, the first raw material includes: silicate ester, phthalate ester, aluminum isopropoxide, and zirconium n-propoxide.
[0043] Optionally, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0044] Optionally, the surfactant includes: cetyltrimethylammonium bromide, polyethylene glycol, polyoxyethylene polyoxypropylene, or a polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer.
[0045] Optionally, it may also include forming an ultraviolet reflective layer on the surface of the emitting layer opposite to the emitting substrate.
[0046] Optionally, the method of forming the ultraviolet reflective layer includes forming one or more stacked ultraviolet reflective sublayers on the surface of the emitting layer opposite to the emitting substrate.
[0047] Optionally, the multilayered ultraviolet reflective sublayer includes a first ultraviolet reflective sublayer to an Mth ultraviolet reflective sublayer stacked sequentially, with the first ultraviolet reflective sublayer located between the Mth ultraviolet reflective sublayer and the emitting layer; M is an integer greater than or equal to 2.
[0048] Optionally, the step of forming the m-th ultraviolet reflective sublayer includes: forming an ultraviolet reflective layer sol solution using a sol-gel method; applying the ultraviolet reflective layer sol solution to the side of the emitting layer opposite to the emitting substrate for the m-th time; and performing a curing treatment on the ultraviolet reflective layer sol solution on the emitting layer for the m-th time to form the m-th ultraviolet reflective sublayer; where m is an integer greater than or equal to 1 and less than or equal to M.
[0049] Optionally, the process of applying the ultraviolet reflective layer sol solution to the side of the emitting layer opposite to the emitting substrate for the mth time includes dip coating, roller coating, or spin coating.
[0050] Optionally, the parameters of the immersion-lifting method include: the immersion speed in the ultraviolet reflective layer sol solution is 3000μm / s~5000μm / s, the lifting speed is 1000μm / s~3000μm / s, and the immersion time in the ultraviolet reflective layer sol solution is 1min~3min.
[0051] Optionally, the temperature of the first curing treatment up to the temperature of the (M-1)th curing treatment is less than the temperature of the Mth curing treatment; the time of the first curing treatment up to the time of the (M-1)th curing treatment is less than the time of the Mth curing treatment.
[0052] Optionally, the temperature difference between the Mth curing treatment and the jth curing treatment is 50℃~200℃; the time difference between the Mth curing treatment and the jth curing treatment is 30min~50min; j is an integer greater than or equal to 1 and less than or equal to M-1.
[0053] Optionally, during the formation of the j-th ultraviolet reflective sublayer, the temperature of the j-th curing treatment is 200℃~300℃, and the time of the j-th curing treatment is 20min-30min.
[0054] Optionally, during the formation of the Mth ultraviolet reflective sublayer, the temperature of the Mth curing treatment is 200℃~500℃, and the time of the Mth curing treatment is 50min~80min.
[0055] Optionally, the step of forming the ultraviolet reflective layer sol solution using the sol-gel method includes: forming a first ultraviolet reflective layer sol solution using the sol-gel method; forming a second ultraviolet reflective layer sol solution using the sol-gel method; and mixing the first ultraviolet reflective layer sol solution and the second ultraviolet reflective layer sol solution and then aging the mixture to form the ultraviolet reflective layer sol solution.
[0056] Optionally, the mass ratio of the first ultraviolet reflective layer sol to the second ultraviolet reflective layer sol is 2:1 to 5:1.
[0057] Optionally, the aging process can be carried out for 7 to 30 days.
[0058] Optionally, the step of forming the first ultraviolet reflective layer sol solution using the sol-gel method includes: mixing titanate or zinc-containing organic salt, alcohol, organic acid and inorganic acid to form the first ultraviolet reflective layer sol solution.
[0059] Optionally, the molar ratio of titanate or zinc organic salt to alcohol is 1:45 to 1:60; the molar ratio of hydrogen ions in organic and inorganic acids to alcohol is 1:60 to 4:60; and the molar ratio of hydrogen ions in organic and inorganic acids to water is 4:0.4 to 4:0.7.
[0060] Optionally, the titanate includes tetraethyl titanate, tetraisopropyl titanate, or tetrabutyl titanate.
[0061] Optionally, the zinc-containing organic salt includes: zinc acetate and zinc diethyldithiocarbamate.
[0062] Optionally, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0063] Optionally, the organic acid includes oxalic acid, acetic acid, or citric acid; the inorganic acid includes hydrochloric acid, nitric acid, or sulfuric acid.
[0064] Optionally, the step of forming the second ultraviolet reflective layer sol solution using the sol-gel method includes: mixing rare earth salts, alcohols and chelating agents to form the second ultraviolet reflective layer sol solution.
[0065] Optionally, the molar ratio of rare earth salt to alcohol is 1:30 to 1:40; the molar ratio of alcohol to chelating agent is 40:0.5 to 40:2.
[0066] Optionally, the rare earth salt includes: carbonate, oxalate, or chloride.
[0067] Optionally, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0068] Optionally, the chelating agent includes: polyacrylic acid, polymaleic anhydride, ethylenediaminetetraacetic acid, or acetylacetone.
[0069] Optionally, the ultraviolet reflective layer sol includes one or more of the following: titanium sol, cerium sol, lanthanum sol, zinc sol, or yttrium sol.
[0070] Optionally, it may also include forming a transparent conductive film on the surface of the ultraviolet reflective layer opposite to the emitting layer.
[0071] Optionally, the method for forming the transparent conductive film includes magnetron sputtering or sol-gel processes.
[0072] Optionally, it further includes: forming a metal reflective layer on the surface of the emitting substrate facing away from the emitting layer; and forming a metal protective layer on the surface of the metal reflective layer facing away from the emitting layer.
[0073] The technical solution of this invention has the following advantages: The optical solar reflector provided by this invention includes an emission layer located on one side surface of the emission substrate. The emissivity of the emission layer is greater than that of the emission substrate. This emission layer can improve the emissivity of the optical solar reflector, thereby improving its heat dissipation performance. Therefore, the optical solar reflector has high heat dissipation performance.
[0074] Furthermore, the emission layer includes one or more stacked emission sub-layers; the emission sub-layer includes an oxide emission sub-layer; the material of the oxide emission sub-layer includes one or more of silicon oxide, titanium oxide, aluminum oxide, zirconium oxide and nickel oxide; the material of the oxide emission sub-layer is an oxide material with high intrinsic emissivity, thus improving the emissivity of the emission layer and thereby improving the heat dissipation performance of the optical solar reflector.
[0075] Furthermore, the emission layer is composed of clustered particles. On the one hand, these clustered particles cannot form an effective scattering source for visible light and infrared bands, and their scattering coefficient is extremely low. On the other hand, the surface of the emission layer, which is formed by the accumulation of clustered particles, has a higher roughness, which increases the specific surface area of the emission layer. Therefore, the emissivity of the emission layer is improved, thereby improving the heat dissipation performance of the optical solar reflector.
[0076] Furthermore, an ultraviolet reflective layer is located on the surface of the emitting layer opposite to the emitting substrate. The ultraviolet reflective layer includes one or more stacked ultraviolet reflective sublayers. The material of the ultraviolet reflective sublayer includes an oxide ultraviolet reflective sublayer. The material of the oxide ultraviolet reflective sublayer has ultraviolet resistance properties that absorb and scatter ultraviolet light, providing ultraviolet protection for the emitting layer and the emitting substrate, and providing excellent protection against atomic oxygen in the environment. This improves the ultraviolet radiation resistance of the optical solar reflector, thereby enhancing the space environment adaptability of the optical solar reflector.
[0077] Furthermore, the optical solar reflector also includes a transparent conductive film located on the surface of the ultraviolet reflective layer facing away from the emitting layer; the transparent conductive film has a certain conductivity, which can prevent the charging and discharging effect of the space environment and play a role in preventing static electricity accumulation. Attached Figure Description
[0078] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0079] Figure 1 This is a schematic diagram of the structure of an optical solar reflector provided in an embodiment of the present invention; Figure 2 A comparison diagram of reflectivity before and after ultraviolet irradiation test on an optical solar reflector, provided as another embodiment of the present invention; Figure 3 A comparison diagram of reflectivity before and after a Co-60 γ-ray irradiation test on an optical solar reflector, provided as an embodiment of the present invention; Figure 4 This is a comparison diagram of the reflectivity of an optical solar reflector before and after a high-low temperature alternating test, provided by an embodiment of the present invention. Figure 5 A flowchart of a method for manufacturing an optical solar reflector according to an embodiment of the present invention; Figure 6 A comparison diagram of transmittance before and after vacuum ultraviolet irradiation when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of an emitting substrate, according to an embodiment of the present invention. Figure 7 A comparison diagram of transmittance before and after Co-60 γ-ray irradiation when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of an emitting substrate, according to an embodiment of the present invention. Figure 8 This is a comparison diagram of transmittance before and after a high and low temperature alternating test when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of an emitting substrate, according to an embodiment of the present invention. Detailed Implementation
[0080] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0081] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0082] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0083] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0084] Example 1 This embodiment provides an optical solar reflector, for reference... Figure 1 ,include: Launch base layer 1; An emission layer 2 is located on one side surface of the emission base layer 1, and the emissivity of the emission layer 2 is greater than that of the emission base layer 1.
[0085] The optical solar reflector provided in this embodiment has an emission layer 2 located on one side surface of the emission base layer 1. The emissivity of the emission layer 2 is greater than that of the emission base layer 1. The emission layer 2 can improve the emissivity of the optical solar reflector, thereby improving its heat dissipation performance. Therefore, the optical solar reflector has high heat dissipation performance.
[0086] In one embodiment, the emitting substrate 1 comprises a flexible substrate; in another embodiment, the emitting substrate comprises a rigid substrate.
[0087] In one embodiment, the thickness of the rigid base layer is 0.05mm to 0.2mm; for example, 0.15mm.
[0088] In one embodiment, the thickness of the flexible substrate is 1μm to 150μm; for example, 50μm, 60μm or 80μm.
[0089] In one embodiment, the flexible base layer is made of perfluoroethylene propylene or polyimide; in other embodiments, the flexible base layer may also be made of other flexible and bendable materials.
[0090] In one embodiment, the rigid base layer is made of quartz glass or cerium-doped glass.
[0091] In one embodiment, the emission layer 2 includes a single emission sublayer; in another embodiment, the emission layer includes multiple stacked emission sublayers.
[0092] In one embodiment, the emitter sublayer comprises an oxide emitter sublayer.
[0093] In one embodiment, the oxide emitter layer is made of one or more of silicon oxide, titanium oxide, aluminum oxide, zirconium oxide, and nickel oxide. The oxide emitter layer is made of an oxide material with high intrinsic emissivity, thus increasing the emissivity of the emitter layer and consequently improving the heat dissipation performance of the optical solar reflector.
[0094] The emission layer 2 is composed of clustered particles. These clustered particles, on the one hand, cannot form an effective scattering source for visible light and infrared wavelengths, exhibiting extremely low scattering coefficients; on the other hand, the surface of the emission layer formed by their accumulation has higher roughness, increasing the specific surface area of the emission layer, thus improving the emissivity of the emission layer and consequently enhancing the heat dissipation performance of the optical solar reflector.
[0095] In one embodiment, the thickness of the emitting layer 2 is 100nm~2000nm, for example 200nm, 300nm or 400nm. If the thickness of the emitting layer 2 is less than 100nm, there is too little oxide material with high intrinsic emissivity in the emitting layer 2, resulting in too little improvement in the emissivity of the emitting layer 2, and thus too little improvement in the heat dissipation function of the optical solar reflector. If the thickness of the emitting layer 2 is greater than 2000nm, the stress of the emitting layer is large, and cracking, peeling and other phenomena are prone to occur, resulting in a significant reduction in service life.
[0096] In one embodiment, the optical solar reflector further includes an ultraviolet reflective layer 3 located on the surface of the emitting layer 2 facing away from the emitting base layer 1, the ultraviolet reflective layer 3 comprising one or more stacked ultraviolet reflective sublayers.
[0097] In one embodiment, the material of the ultraviolet reflective sublayer includes an oxide ultraviolet reflective sublayer.
[0098] In one embodiment, the material of the oxide ultraviolet reflective sublayer includes one or a combination of titanium oxide, cerium oxide, yttrium oxide, lanthanum oxide, and zinc oxide. The material of the oxide ultraviolet reflective sublayer exhibits ultraviolet resistance properties, absorbing and scattering ultraviolet light, thus providing ultraviolet protection for the emitting layer 2 and the emitting substrate 1, and offering excellent protection against atomic oxygen in the environment. This improves the atomic oxygen resistance of the optical solar reflector, thereby enhancing its space environment adaptability.
[0099] In one embodiment, the thickness of the ultraviolet reflective layer 3 is 50nm~300nm, for example 80nm, 100nm or 100nm. If the thickness of the ultraviolet reflective layer 3 is less than 50nm, the ultraviolet reflective layer 3 provides insufficient protection against ultraviolet radiation to the emitting layer and the emitting substrate, provides insufficient protection against atomic oxygen in the environment, provides insufficient protection against ultraviolet radiation to the optical solar reflector, and consequently provides insufficient protection against ultraviolet radiation to the optical solar reflector. If the thickness of the ultraviolet reflective layer 3 is greater than 300nm, the thickness of the ultraviolet reflective layer 3 is too large, resulting in insufficient improvement in the emissivity of the optical solar reflector.
[0100] In one embodiment, the optical solar reflector further includes a transparent conductive film 4 located on the surface of the ultraviolet reflective layer 3 facing away from the emitting layer 2. The transparent conductive film 4 has a certain degree of conductivity, which can prevent the charging and discharging effects of the space environment and play a role in preventing static electricity accumulation.
[0101] In one embodiment, the transparent conductive film 4 is an ITO thin film, where ITO refers to indium tin oxide.
[0102] In one embodiment, the thickness of the transparent conductive film 4 is 5nm to 50nm, for example, 5nm, 20nm or 50nm; if the thickness of the transparent conductive film is less than 5nm, the transparent conductive film 4 plays a very small role in preventing static electricity accumulation; if the thickness of the transparent conductive film 4 is greater than 50nm, the thickness of the transparent conductive film 4 is too large, and the degree to which it improves the emissivity of the optical solar reflector is small.
[0103] In one embodiment, the optical solar reflector further includes a metal reflective layer 5, which is located on the surface of the base layer 1 facing away from the base layer 2.
[0104] In one embodiment, the thickness of the metal reflective layer 5 is 50nm to 500nm, for example, 100nm.
[0105] In one embodiment, the material of the metal reflective layer 5 includes one or more of the following: silver, aluminum, copper, bismuth, germanium, and chromium.
[0106] In one embodiment, the optical solar reflector further includes a metal protective layer 6, which is located on the surface of the metal reflective layer 5 facing away from the reflective substrate 1. The metal protective layer 6 primarily protects the metal reflective layer, which is prone to slow oxidation when exposed to air for extended periods.
[0107] In one embodiment, the thickness of the metal protective layer 6 is 10nm to 300nm, for example, 100nm.
[0108] In one embodiment, the material of the metal protective layer 6 includes a nickel-based alloy.
[0109] In this embodiment, the materials of the ultraviolet reflective layer and the emitting layer both include inorganic oxides, which have comprehensive resistance to space irradiation / ultraviolet radiation and other space environments, broadening the range of various orbital space environments, greatly improving the reliability of spacecraft space applications, and also greatly extending the spacecraft's space operational lifespan.
[0110] In one specific embodiment, the emitting substrate of the optical solar reflector is a rigid substrate made of cerium-doped glass; the emitting layer located on one side of the emitting substrate comprises three stacked emitting sub-layers made of silicon dioxide; an ultraviolet reflective layer located on the surface of the emitting layer facing away from the emitting substrate comprises one ultraviolet reflective sub-layer made of a combination of titanium oxide and cerium oxide; a transparent conductive film is also present on the surface of the ultraviolet reflective layer facing away from the emitting layer; a metal reflective layer located on the surface of the emitting substrate facing away from the emitting layer is made of silver; and a metal protective layer on the surface of the metal reflective layer facing away from the emitting substrate is made of a nickel-based alloy.
[0111] Figure 2 This is a comparison of the reflectivity of the optical solar reflector provided in this embodiment before and after vacuum ultraviolet irradiation, where the total ultraviolet irradiation dose in the vacuum ultraviolet irradiation test was 1500 ESH. Figure 2 The horizontal axis represents the wavelength at which the optical solar reflector is irradiated with vacuum ultraviolet light. Figure 2 The vertical axis represents the reflectivity of the optical solar reflector before and after vacuum ultraviolet irradiation. It can be seen that the optical solar reflector provided in this embodiment provides excellent protection against vacuum ultraviolet irradiation.
[0112] Figure 3 This image shows a comparison of the reflectivity of the optical solar reflector provided in this embodiment before and after Co-60 gamma-ray irradiation. The total irradiation dose in the Co-60 gamma-ray irradiation experiment was 1.0. 10 9 rad, Figure 3 The horizontal axis represents the wavelength at which the optical solar reflector is irradiated with Co-60 γ-rays. Figure 3 The vertical axis represents the reflectivity of the optical solar reflector before and after Co-60 gamma-ray irradiation. It can be seen that the optical solar reflector provided in this embodiment provides excellent protection against Co-60 gamma-ray irradiation.
[0113] Figure 4 This is a comparison chart of the reflectivity of the optical solar reflector provided in this embodiment before and after the high and low temperature alternating test. Figure 4 The horizontal axis represents the wavelength at which the optical solar reflector undergoes alternating high and low temperatures. Figure 4 The vertical axis represents the reflectivity of the optical solar reflector before and after undergoing alternating high and low temperatures. The experimental conditions for alternating high and low temperatures were -196℃ to 100℃, with 100 cycles of alternation. This demonstrates that the optical solar reflector provided in this embodiment can withstand the alternating high and low temperatures of space.
[0114] Tests showed that the emissivity ε of the optical solar reflector prepared in this embodiment was increased to 0.85, and the absorptivity was 0.08.
[0115] Example 2 This embodiment provides a method for manufacturing an optical solar reflector, referring to... Figure 5 This includes the following steps: Step S1: Provide the launch base layer; Step S2: An emission layer is formed on one side surface of the emission base layer, wherein the emissivity of the emission layer is greater than that of the emission base layer.
[0116] In step S2, specifically, the method of forming the emission layer includes: forming one or more stacked emission sublayers on one side surface of the emission base layer.
[0117] During the formation of the emission layer, multiple layers of emission sub-layers are formed on one side surface of the emission base layer. This helps to reduce the edge effect of the emission layer and thus improve the uniformity of the thickness of the emission layer.
[0118] In one embodiment, the multilayered emitter sublayers include a first emitter sublayer to an Nth emitter sublayer stacked sequentially, wherein the first emitter sublayer is located between the Nth emitter sublayer and the emitter base layer; N is an integer greater than or equal to 2.
[0119] In one embodiment, the step of forming the nth emitter sublayer includes: forming an emitter sol solution using a sol-gel method; applying the emitter sol solution to one side surface of the emitter substrate for the nth time; and performing a curing treatment on the emitter sol solution on the emitter substrate for the nth time to form the nth emitter sublayer; where n is an integer greater than or equal to 1 and less than or equal to N.
[0120] In one embodiment, the thickness of the nth emitting sublayer is 100nm~300nm, for example 200nm. If the thickness of the nth emitting sublayer is less than 100nm, the thickness of the nth emitting sublayer is too small, and the degree to which the fabrication efficiency of the optical solar reflector is improved is low. If the thickness of the nth emitting sublayer is greater than 300nm, the thickness of the nth emitting sublayer is too large, and the degree to which the edge effect of the emitting layer is reduced is reduced, and the degree to which the uniformity of the thickness of the emitting layer is improved is reduced.
[0121] In one embodiment, the temperatures of the first curing treatment to the (N-1)th curing treatment are all lower than the temperature of the Nth curing treatment. The lower temperatures of the first curing treatment to the (N-1)th curing treatment are suitable for initially curing the corresponding emitter sublayers, which helps to improve the manufacturing efficiency of the optical solar reflector while reducing costs. The higher temperature of the Nth curing treatment is suitable for fully curing the first emitter sublayer to the Nth emitter sublayer.
[0122] In one embodiment, the time for the first curing process to the (N-1)th curing process is shorter than the time for the Nth curing process. The shorter time for the first curing process to the (N-1)th curing process is suitable for initially curing the corresponding emitter sublayers, which helps to improve the manufacturing efficiency of the optical solar reflector while reducing costs. The longer time for the Nth curing process is suitable for fully curing the first emitter sublayer to the Nth emitter sublayer.
[0123] In one embodiment, the temperature difference between the Nth curing treatment and the kth curing treatment is 50°C to 200°C, for example, 180°C, where k is an integer greater than or equal to 1 and less than or equal to N-1. This is beneficial for improving the manufacturing efficiency of the optical solar reflector while reducing costs.
[0124] In one embodiment, the time difference between the Nth curing treatment and the kth curing treatment is 30 to 50 minutes, for example, 45 minutes, where k is an integer greater than or equal to 1 and less than or equal to N-1. This is beneficial for improving the fabrication efficiency of the high-emission optical solar reflector while reducing costs.
[0125] In one embodiment, during the formation of the k-th emitter layer, the temperature of the k-th curing process is 200°C to 300°C, for example, 250°C. Here, k is an integer greater than or equal to 1 and less than or equal to N-1.
[0126] In one embodiment, during the formation of the k-th emitter sublayer, the time for the k-th curing process is 20 min to 30 min, for example, 25 min. Here, k is an integer greater than or equal to 1 and less than or equal to N-1.
[0127] In one embodiment, during the formation of the Nth emitter sublayer, the temperature of the Nth curing process is 200°C to 500°C, for example, 450°C.
[0128] In one embodiment, during the formation of the Nth emitter layer, the time for the Nth curing process is 50 to 80 minutes, for example, 60 minutes. If the time for the Nth curing process is less than 50 minutes, the curing time of the emitter layer is too short, resulting in a small improvement in the degree of complete curing of the emitter layer. If the time for the Nth curing process is more than 80 minutes, the curing time of the emitter layer is too long, resulting in a small improvement in the fabrication efficiency of the optical solar reflector.
[0129] In one embodiment, the process of applying the emissive layer sol to one side surface of the emissive substrate for the nth time includes an dip-coating method. Specifically, before forming the nth emissive sublayer, a first protective film is formed on the other side surface of the emissive substrate. The first protective film adheres tightly to the emissive substrate to prevent air bubbles from forming at the edges. During the nth application of the emissive layer sol to one side surface of the emissive substrate using the dip-coating method, the first protective film serves as a protection. After the nth application of the emissive layer sol to one side surface of the emissive substrate, the first protective film is removed. It should be noted that a first protective film needs to be formed before each application of the emissive layer sol to one side surface of the emissive substrate.
[0130] In one embodiment, the parameters for the dip-coating method used for the nth coating include: the immersion speed in the sol solution of the emitting layer is 3000 μm / s to 5000 μm / s, for example, 3500 μm / s; if the immersion speed in the sol solution of the emitting layer is less than 3000 μm / s, the rate of forming the emitting sublayer is too small, and the degree to which the fabrication efficiency of the optical solar reflector is improved is too small; if the immersion speed in the sol solution of the emitting layer is greater than 5000 μm / s, the immersion speed in the sol solution of the emitting layer is too large, which is not conducive to subsequent coating.
[0131] In one embodiment, the parameters for the dip-coating method used for the nth coating include: a dipping speed of 1000 μm / s to 2000 μm / s, for example, 1500 μm / s. If the dipping speed is lower than 1000 μm / s, the thickness of the emitted sublayer is too thin, requiring multiple dipping and curing processes during the formation of the emitted layer, thus reducing the efficiency of the optical solar reflector fabrication. If the dipping speed is higher than 2000 μm / s, the thickness of the emitted sublayer is too thick, resulting in less reduction of the edge effect of the emitted sublayer and a lower degree of improvement in the uniformity of the emitted layer.
[0132] In one embodiment, the parameters of the dip-coating method used for the nth coating include: the immersion time in the sol solution of the emitting layer is 1 min to 3 min, for example, 2 min; if the immersion time in the sol solution of the emitting layer is less than 1 min, the improvement in the structural stability of the emitting layer is low; if the immersion time of the emitting substrate in the sol solution of the emitting layer is more than 3 min, the improvement in the fabrication efficiency of the optical solar reflector is too small.
[0133] In one embodiment, the step of forming an emission layer sol using the sol-gel method includes: providing a first raw material and an alcohol, an acid solution, and a surfactant; dissolving the surfactant in the alcohol and stirring uniformly; after dissolving the surfactant in the alcohol and stirring uniformly, adding the acid solution and the first raw material and stirring; and after adding the acid solution and the first raw material and stirring, performing an aging treatment to form an emission layer sol.
[0134] In one embodiment, in the step of adding the acid solution and the first raw material and stirring, the stirring time is 6h~24h, for example 10h; if the stirring time is less than 6h, the degree of sufficient reaction between the acid solution and the first raw material is low; if the stirring time is more than 24h, the degree of improvement in the preparation efficiency of the optical solar reflector is too small.
[0135] In one embodiment, the aging process for forming the emitter sol is carried out for a period of 7 to 30 days, for example, 8 days.
[0136] In one embodiment, the molar ratio of the first raw material to the alcohol is 1:18 to 1:25, for example, 1:20.
[0137] In one embodiment, the molar ratio of alcohol to acid solution is 0.1~25:0.2~25, for example 0.15:25.
[0138] In one embodiment, the molar ratio of acid solution to water is 0.2:8 to 0.2:12, for example, 0.2:10.
[0139] In one embodiment, the acid solution includes: hydrochloric acid solution, nitric acid solution, or acetic acid solution.
[0140] In one embodiment, the molar concentration of the acid solution is 0.12 mol / L to 0.18 mol / L, for example, 0.16 mol / L.
[0141] In one embodiment, the first raw material includes: silicate ester, titanate ester, aluminum isopropoxide, or zirconium n-propoxide.
[0142] In one embodiment, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0143] In one embodiment, the surfactant includes: cetyltrimethylammonium bromide, polyethylene glycol, polyoxyethylene polyoxypropylene, or a polyoxyethylene-polyoxypropylene-polyoxyethylene triblock copolymer.
[0144] In another embodiment, the ultraviolet reflective layer sol solution comprises one or more of the following: titanium oxide, cerium oxide, yttrium oxide, lanthanum oxide, and zinc oxide sol solutions.
[0145] In one embodiment, the method for fabricating the optical solar reflector further includes forming an ultraviolet reflective layer on the surface of the emitting layer opposite to the emitting substrate.
[0146] In one embodiment, the method of forming the ultraviolet reflective layer includes forming one or more stacked ultraviolet reflective sublayers on the side surface of the emitting layer opposite to the emitting substrate.
[0147] In one embodiment, the multilayered ultraviolet reflective sublayers include a first ultraviolet reflective sublayer to an Mth ultraviolet reflective sublayer stacked sequentially, with the first ultraviolet reflective sublayer located between the Mth ultraviolet reflective sublayer and the emitting layer; M is an integer greater than or equal to 2.
[0148] In one embodiment, the step of forming the m-th ultraviolet reflective sublayer includes: forming an ultraviolet reflective layer sol solution using a sol-gel method; applying the ultraviolet reflective layer sol solution to the side of the emitting layer opposite to the emitting substrate for the m-th time; and performing a curing treatment on the ultraviolet reflective layer sol solution on the emitting layer for the m-th time to form the m-th ultraviolet reflective sublayer; where m is an integer greater than or equal to 1 and less than or equal to M.
[0149] In one embodiment, the process of applying the UV reflective layer sol solution for the mth time to the side of the emitting layer facing away from the emitting substrate includes an dip-coating method. Specifically, before forming the mth UV reflective sublayer, a second protective film is formed on the surface of the emitting substrate facing away from the emitting layer. The second protective film adheres tightly to the emitting substrate to prevent air bubbles from forming at the edges. During the mth time of applying the UV reflective layer sol solution to the side of the emitting layer facing away from the emitting substrate using the dip-coating method, the second protective film serves as a protection. After the mth time of applying the UV reflective layer sol solution to the side of the emitting layer facing away from the emitting substrate, the second protective film is removed. It should be noted that a second protective film needs to be formed before each application to the side of the emitting layer facing away from the emitting substrate.
[0150] In one embodiment, the parameters for the dip-coating method used for the m-th coating include: the immersion speed in the UV reflective layer sol solution is 3000 μm / s to 5000 μm / s, for example, 3500 μm / s.
[0151] In one embodiment, the parameters for the dip-coating method used in the m-th coating include: a coating speed of 1000 μm / s to 3000 μm / s, for example, 2000 μm / s. If the coating speed is less than 1000 μm / s, the rate of forming the ultraviolet reflective layer is too low, resulting in insufficient improvement in the fabrication efficiency of the optical solar reflector. If the coating speed is greater than 3000 μm / s, the rate of forming the ultraviolet reflective layer is too high, leading to poor uniformity of the ultraviolet reflective layer.
[0152] In one embodiment, the parameters for the dip-coating method used for the m-th coating include: the immersion time in the UV reflective layer sol solution is 1 min to 3 min, for example, 2 min.
[0153] In one embodiment, the temperatures of the first curing treatment up to the (M-1)th curing treatment are all lower than the temperature of the Mth curing treatment; and the times of the first curing treatment up to the (M-1)th curing treatment are all lower than the time of the Mth curing treatment. This is beneficial for improving the manufacturing efficiency of the optical solar reflector while reducing costs.
[0154] In one embodiment, the temperature difference between the Mth curing treatment and the jth curing treatment is 50°C to 200°C, for example, 150°C, and the time difference between the Mth curing treatment and the jth curing treatment is 30 min to 50 min, for example, 40 min; j is an integer greater than or equal to 1 and less than or equal to M-1.
[0155] In one embodiment, during the formation of the Mth ultraviolet reflective sublayer, the temperature of the Mth curing process is 200°C to 500°C, for example, 300°C.
[0156] In one embodiment, the curing time for the Mth curing process is 50-80 minutes, for example, 60 minutes. If the curing time for the Mth curing process is less than 50 minutes, the curing time of the ultraviolet reflective layer is too short, resulting in a small improvement in the degree of complete curing of the ultraviolet reflective layer. If the curing time for the Mth curing process is more than 80 minutes, the curing time of the ultraviolet reflective layer is too long, resulting in a small improvement in the fabrication efficiency of the optical solar reflector.
[0157] In one embodiment, the curing of the multiple layers of ultraviolet reflective sublayers in the ultraviolet reflective layer is a single simultaneous curing; in other embodiments, curing is performed after each ultraviolet reflective sublayer is formed.
[0158] In one embodiment, the step of forming an ultraviolet reflective layer sol solution using the sol-gel method includes: forming a first ultraviolet reflective layer sol solution using the sol-gel method; forming a second ultraviolet reflective layer sol solution using the sol-gel method; and aging the first ultraviolet reflective layer sol solution and the second ultraviolet reflective layer sol solution together to form the ultraviolet reflective layer sol solution.
[0159] In one embodiment, the mass ratio of the first ultraviolet reflective layer sol to the second ultraviolet reflective layer sol is 2:1 to 5:1, for example, 3:1.
[0160] In one embodiment, the aging process for forming the UV reflective layer sol is carried out for a period of 7 to 30 days, for example, 7 days.
[0161] In one embodiment, the step of forming the first ultraviolet reflective layer sol solution using the sol-gel method includes: mixing titanate, alcohol, organic acid and inorganic acid to form the first ultraviolet reflective layer sol solution.
[0162] In one embodiment, the molar ratio of titanate ester to alcohol is 1:45 to 1:60, for example 1:50; the molar ratio of hydrogen ions in organic and inorganic acids to alcohol is 1:60 to 4:60, for example 2:60; and the molar ratio of hydrogen ions in organic and inorganic acids to water is 4:0.4 to 4:0.7, for example 4:0.6.
[0163] In another embodiment, a zinc-containing organic salt, alcohol, organic acid, and inorganic acid are mixed to form the first ultraviolet reflective layer sol solution.
[0164] In one embodiment, the molar ratio of the zinc-containing organic salt to the alcohol is 1:45 to 1:60, for example, 1:50; the molar ratio of hydrogen ions in the organic acid and inorganic acid to the alcohol is 1:60 to 4:60, for example, 2:60; and the molar ratio of hydrogen ions in the organic acid and inorganic acid to water is 4:0.4 to 4:0.7, for example, 4:0.6.
[0165] In one embodiment, the titanate includes tetraethyl titanate, tetraisopropyl titanate, or tetrabutyl titanate.
[0166] In one embodiment, the zinc-containing organic salt includes: zinc acetate and zinc diethyldithiocarbamate.
[0167] In one embodiment, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0168] In one embodiment, the organic acid includes oxalic acid, acetic acid, or citric acid; and the inorganic acid includes hydrochloric acid, nitric acid, or sulfuric acid.
[0169] In one embodiment, the step of forming the second ultraviolet reflective layer sol solution using the sol-gel method includes: mixing rare earth salts, alcohols, and chelating agents to form the second ultraviolet reflective layer sol solution.
[0170] In one embodiment, the molar ratio of rare earth salt to alcohol is 1:30 to 1:40, for example 1:35; the molar ratio of alcohol to chelating agent is 40:0.5 to 40:2, for example 40:1.
[0171] In one embodiment, the rare earth salt includes: carbonate, oxalate, or chloride.
[0172] In one embodiment, the alcohol includes methanol, ethanol, isopropanol, or butanol.
[0173] In one embodiment, the chelating agent includes: polyacrylic acid, polymaleic anhydride, ethylenediaminetetraacetic acid, or acetylacetone.
[0174] In another embodiment, the ultraviolet reflective layer sol includes one or a combination of titanium sol, cerium sol, lanthanum sol, zinc sol and yttrium sol.
[0175] The optical solar reflector fabrication method provided in this embodiment uses a sol-gel method to form the emission layer. This method can directly form the emission layer on emission substrates of different shapes and materials. The sol-gel method helps to improve the adhesion between the emission layer and the emission substrate, thereby improving the emissivity of the emission layer and thus improving the heat dissipation performance of the optical solar reflector.
[0176] In one embodiment, the method for fabricating the optical solar reflector further includes: forming a transparent conductive film on the surface of the ultraviolet reflective layer facing away from the emitting layer.
[0177] In one embodiment, the method for forming the transparent conductive film includes a magnetron sputtering process or a sol-gel process; in other embodiments, the method for forming the transparent conductive film may also include other deposition processes.
[0178] In one embodiment, the temperature at which the transparent conductive film is formed is 70°C to 100°C, for example, 80°C.
[0179] In one embodiment, the transparent conductive film is further subjected to an annealing treatment at a temperature of 400°C to 500°C, for example, 450°C. The annealing time is 90 min to 150 min, for example, 120 min.
[0180] In one embodiment, the method for fabricating the optical solar reflector further includes: forming a metal reflective layer on the side surface of the emitting substrate facing away from the emitting layer, and forming a metal protective layer on the side surface of the metal reflective layer facing away from the emitting layer.
[0181] In one specific embodiment, the material of the emitting substrate is cerium-doped glass; an emitting layer is formed on one side surface of the cerium-doped glass, and an ultraviolet reflective layer is formed on the side surface of the emitting layer opposite to the emitting substrate. The steps of forming the emitting layer include: forming three stacked emitting sub-layers on one side surface of the cerium-doped glass, specifically, forming an emitting layer sol solution using a sol-gel method; firstly coating the emitting layer sol solution onto one side surface of the emitting substrate, and firstly curing the emitting layer sol solution on the emitting substrate to form the first emitting sub-layer; secondly coating the emitting layer sol solution onto the side surface of the first emitting sub-layer opposite to the emitting substrate, and secondly curing the emitting layer sol solution on the first emitting sub-layer to form the second emitting sub-layer; and then... The emissive sol is coated a third time on the surface of the second emissive sublayer facing away from the emissive substrate. The emissive sol on the second emissive sublayer is then cured a third time to form the third emissive sublayer. During the formation of the first and second emissive sublayers, the curing temperature is 300°C and the curing time is 20 minutes. During the formation of the third emissive sublayer, the curing temperature is 400°C and the curing time is 80 minutes. The process of coating the emissive sol on one side of the emissive substrate includes an dip-coating method. The parameters of the dip-coating method include: an immersion speed of 4500 μm / s in the emissive sol, a lifting speed of 1500 μm / s, and a soaking time of 3 minutes for the emissive substrate in the emissive sol. The steps for forming the sol-gel method for the emission layer include: dissolving a surfactant in alcohol and stirring uniformly; then, sequentially adding a dilute acid with a molar concentration of 0.15 mol / L and tetraethyl orthosilicate and stirring again; and aging for 7 days to form the emission layer sol. The steps for forming the ultraviolet reflective layer include: forming an ultraviolet reflective sublayer on the surface of the emission layer facing away from the emission substrate; forming the ultraviolet reflective sublayer includes: forming an ultraviolet reflective layer sol using the sol-gel method; applying the ultraviolet reflective layer sol to the side of the emission layer facing away from the emission substrate; and performing a curing treatment on the ultraviolet reflective layer sol on the emission layer to form the ultraviolet reflective sublayer. The process of coating the ultraviolet reflective layer sol solution onto the side of the emitting layer opposite to the emitting substrate in one step includes the dip-coating method; the parameters of the dip-coating method include: the immersion speed in the ultraviolet reflective layer sol solution is 5000 μm / s, the lifting speed is 1500 μm / s, and the immersion time in the ultraviolet reflective layer sol solution is 3 min.The steps for forming a UV-reflective layer sol solution using the sol-gel method include: forming a first UV-reflective layer sol solution using the sol-gel method; forming a second UV-reflective layer sol solution using the sol-gel method, wherein the first UV-reflective layer sol solution and the second UV-reflective layer sol solution are mixed and aged to form the UV-reflective layer sol solution; the mass ratio of the first UV-reflective layer sol solution to the second UV-reflective layer sol solution is 2:1; the formation of the first UV-reflective layer sol solution includes: adding an organic acid to anhydrous ethanol and mixing evenly, then adding tetratetrate titanate and stirring evenly; then continuing to add organic acid and dilute hydrochloric acid, reacting for 1 hour and stopping stirring, aging for 7 days to form the first UV-reflective layer sol solution; the formation of the second UV-reflective layer sol solution includes: dissolving cerium salt in anhydrous ethanol, mixing evenly, adding a chelating agent, reacting for 6 hours and stopping stirring, aging for 10 days to form the second UV-reflective layer sol solution.
[0182] Tests showed that, using the optical solar reflector fabrication method provided in this embodiment, the emissivity ε was increased to 0.89 when an emitting layer and an ultraviolet reflective layer were sequentially formed on one side of the emitting substrate.
[0183] Figure 6 This image shows a comparison of transmittance before and after vacuum ultraviolet irradiation when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of the emitting substrate using the optical solar reflector fabrication method provided in this embodiment. The total ultraviolet irradiation dose in the vacuum ultraviolet irradiation test was 1500 ESH. Figure 6 The horizontal axis represents the wavelength of vacuum ultraviolet irradiation when only the base layer, the emitting layer, and the ultraviolet reflective layer are included. Figure 6 The vertical axis represents the transmittance before and after vacuum ultraviolet irradiation when only the base layer, the emitting layer, and the ultraviolet reflective layer are included. It can be seen that the optical solar reflector fabrication method provided in this embodiment, which sequentially forms the emitting layer and the ultraviolet reflective layer on one side of the emitting base layer, provides excellent protection against vacuum ultraviolet irradiation.
[0184] Figure 7 This image shows a comparison of transmittance before and after Co-60 γ-ray irradiation when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of the emitting substrate using the optical solar reflector fabrication method provided in this embodiment. The total irradiation dose in the Co-60 γ-ray irradiation experiment was 1.0. 109 rad, Figure 7 The horizontal axis represents the wavelength of Co-60 γ-ray irradiation when only the base layer, the emitting layer, and the ultraviolet reflector layer are included. Figure 7The vertical axis represents the transmittance before and after Co-60 γ-ray irradiation when only the emitting substrate, emitting layer, and ultraviolet reflective layer are included. It can be seen that the optical solar reflector fabrication method provided in this embodiment, which sequentially forms the emitting layer and ultraviolet reflective layer on one side of the emitting substrate, provides excellent protection against Co-60 γ-ray irradiation.
[0185] Figure 8 This image shows a comparison of transmittance before and after a high-low temperature alternating test when an emitting layer and an ultraviolet reflective layer are sequentially formed on one side of the emitting substrate using the optical solar reflector fabrication method provided in this embodiment. Figure 8 The horizontal axis represents the wavelength used in the high and low temperature alternating test when only the base layer, the emitting layer, and the ultraviolet reflective layer are included. Figure 8 The vertical axis represents the transmittance before and after high-low temperature alternation when only the base layer, the emitting layer, and the ultraviolet reflective layer are included. The experimental conditions for the high-low temperature alternation test were -196℃ to 100℃, with 100 cycles of high-low temperature alternation. It can be seen that the optical solar reflector fabrication method provided in this embodiment, when the emitting layer and the ultraviolet reflective layer are sequentially formed on one side of the emitting base layer, can withstand the high-low temperature alternation environment in space.
[0186] The method for preparing the optical solar reflector provided in this embodiment can directly deposit a film on the emitting substrate, without being limited by the shape or type of the emitting substrate, and has the advantages of large-scale production and simple process flow.
[0187] The method for fabricating an optical solar reflector provided in this embodiment can increase the emissivity of the reflector from 0.81 to over 0.85, an increase of more than 4%. This increase in emissivity can improve the heat dissipation efficiency of spacecraft by more than 15%, increasing the spacecraft's payload and extending its service life. Furthermore, because the optical solar reflector provided in this embodiment has an ultraviolet reflective layer, it maintains high emissivity without compromising its adaptability to the space environment. In addition, introducing the sol-gel coating method into the field of aerospace coating not only saves production costs but also broadens the possibilities for aerospace coating methods, resulting in significant economic and social benefits.
[0188] The parts of this embodiment that are the same as the previous embodiment will not be described in detail.
[0189] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. An optical solar reflector, characterized in that, include: Launching from the grassroots level; An emitting layer located on one side surface of the emitting substrate has an emissivity greater than that of the emitting substrate. The emitting layer is composed of clustered particles and its material includes inorganic oxides. The optical solar reflector is used in the space environment.
2. The optical solar reflector according to claim 1, characterized in that, The emission layer includes one or more stacked emission sub-layers, and the emission sub-layers include oxide emission sub-layers.
3. The optical solar reflector according to claim 2, characterized in that, The material of the oxide emitter layer includes one or a combination of silicon dioxide, titanium dioxide, aluminum oxide and nickel oxide.
4. The optical solar reflector according to claim 1, characterized in that, The thickness of the emission layer is 100nm~2000nm.
5. The optical solar reflector according to claim 1, characterized in that, Also includes: An ultraviolet reflective layer is located on the surface of the emitting layer opposite to the emitting base layer, the ultraviolet reflective layer comprising one or more stacked ultraviolet reflective sublayers.
6. The optical solar reflector according to claim 5, characterized in that, The material of the ultraviolet reflective sublayer includes an oxide ultraviolet reflective sublayer.
7. The optical solar reflector according to claim 6, characterized in that, The material of the oxide ultraviolet reflective sublayer includes one or a combination of titanium dioxide, cerium oxide, or zinc oxide.
8. The optical solar reflector according to claim 5, characterized in that, The thickness of the ultraviolet reflective layer is 50nm~300nm.
9. The optical solar reflector according to claim 5, characterized in that, Also includes: A transparent conductive film located on the surface of the ultraviolet reflective layer facing away from the emitting layer.
10. The optical solar reflector according to claim 9, characterized in that, The thickness of the transparent conductive film is 5nm~50nm.
11. The optical solar reflector according to claim 1, characterized in that, Also includes: A metal reflective layer is located on the surface of the emitting substrate opposite to the emitting layer. The optical solar reflector further includes a metal protective layer located on the surface of the metal reflective layer facing away from the base layer.
12. The optical solar reflector according to claim 11, characterized in that, The materials of the metal reflective layer include: silver, aluminum, copper, bismuth, germanium or chromium; the materials of the metal protective layer include: nickel-based alloys.
13. The optical solar reflector according to claim 1, characterized in that, The base layer for launching includes a flexible base layer or a rigid base layer.
14. The optical solar reflector according to claim 13, characterized in that, The thickness of the flexible base layer is 1μm to 150μm; the thickness of the rigid base layer is 0.05mm to 0.2mm.
15. The optical solar reflector according to claim 13, characterized in that, The flexible base layer is made of poly(fluoroethylene propylene) or polyimide; the rigid base layer is made of quartz glass or cerium-doped glass.
16. A method for manufacturing an optical solar reflector, characterized in that, include: Provide launch base; An emission layer is formed on one side surface of the emission base layer. The emission layer has a higher emissivity than the emission base layer. The emission layer is composed of clustered particles. The material of the emission layer includes inorganic oxides. The optical solar reflector is used in the space environment.
17. The method for manufacturing an optical solar reflector according to claim 16, characterized in that, A method for forming an emission layer on one side surface of the emission substrate includes: forming one or more stacked emission sub-layers on one side surface of the emission substrate; the stacked emission sub-layers include a first emission sub-layer to an Nth emission sub-layer stacked sequentially, wherein the first emission sub-layer is located between the Nth emission sub-layer and the emission substrate; N is an integer greater than or equal to 2.
18. The method for manufacturing an optical solar reflector according to claim 17, characterized in that, The steps for forming the nth emitter sublayer include: forming an emitter layer sol solution using a sol-gel method; applying the emitter layer sol solution to one side surface of the emitter substrate for the nth time; and performing a curing treatment on the emitter layer sol solution on the emitter substrate for the nth time to form the nth emitter sublayer; where n is an integer greater than or equal to 1 and less than or equal to N.
19. The method for manufacturing an optical solar reflector according to claim 18, characterized in that, The process of coating the emissive layer sol onto one side surface of the emissive substrate includes dip coating, roller coating, or spin coating.
20. The method for manufacturing an optical solar reflector according to claim 19, characterized in that, The parameters of the immersion-lifting method include: the immersion speed in the emissive layer sol is 3000μm / s~5000μm / s, the lifting speed is 1000μm / s~2000μm / s, and the immersion time in the emissive layer sol is 1min~3min.
21. The method for manufacturing an optical solar reflector according to claim 18, characterized in that, The temperatures of the first curing treatment to the (N-1)th curing treatment are all lower than the temperature of the Nth curing treatment; the times of the first curing treatment to the (N-1)th curing treatment are all lower than the times of the Nth curing treatment.
22. The method for manufacturing an optical solar reflector according to claim 21, characterized in that, The temperature difference between the Nth curing treatment and the kth curing treatment is 50℃~200℃; the time difference between the Nth curing treatment and the kth curing treatment is 30min~50min; k is an integer greater than or equal to 1 and less than or equal to N-1.
23. The method for manufacturing an optical solar reflector according to claim 22, characterized in that, During the formation of the k-th emitter sublayer, the temperature of the k-th curing treatment is 200℃~300℃, and the time of the k-th curing treatment is 20min~30min; During the formation of the Nth emitter layer, the temperature of the Nth curing treatment is 200℃~500℃, and the time of the Nth curing treatment is 50min~80min.
24. The method for manufacturing an optical solar reflector according to claim 18, characterized in that, The emitter layer sol includes one or a combination of silica sol, titanium sol, aluminum sol, zirconium sol, or nickel sol.
25. The method for manufacturing an optical solar reflector according to claim 18, characterized in that, The steps for forming the emission layer sol using the sol-gel method include: Provide the first raw materials and alcohol, acid solutions and surfactants; The surfactant was dissolved in alcohol and stirred evenly. After dissolving the surfactant in alcohol and stirring it evenly, an acid solution and the first raw material are added and stirred. After adding acid solution and the first raw material and stirring, the mixture is aged to form an emission layer sol.
26. The method for manufacturing an optical solar reflector according to claim 25, characterized in that, In the step of adding acid solution and the first raw material and stirring, the stirring time is 6h~24h; the aging time is 7 days~30 days.
27. The method for manufacturing an optical solar reflector according to claim 25, characterized in that, The molar ratio of the first raw material to alcohol is 1:18 to 1:25; the molar ratio of alcohol to acid solution is 0.1 to 25: 0.2 to 25; and the molar ratio of acid solution to water is 0.2: 8 to 0.2:
12.
28. The method for manufacturing an optical solar reflector according to claim 26, characterized in that, The acid solution includes hydrochloric acid solution, nitric acid solution, or acetic acid solution, and the molar concentration of the acid solution is 0.12 mol / L to 0.18 mol / L; The first raw material includes: silicate ester, phthalate ester, aluminum isopropoxide, and zirconium n-propoxide; The alcohols include: methanol, ethanol, isopropanol, or butanol; The surfactants include: cetyltrimethylammonium bromide, polyethylene glycol, polyoxyethylene polyoxypropylene, or polyethylene oxide-polyoxypropylene-polyoxyethylene triblock copolymer.
29. The method for manufacturing an optical solar reflector according to claim 16, characterized in that, Also includes: An ultraviolet reflective layer is formed on the surface of the emitting layer that is away from the emitting substrate.
30. The method for manufacturing an optical solar reflector according to claim 29, characterized in that, The method of forming the ultraviolet reflective layer includes: forming one or more stacked ultraviolet reflective sublayers on the side surface of the emitting layer facing away from the emitting substrate; the stacked ultraviolet reflective sublayers include a first ultraviolet reflective sublayer to an Mth ultraviolet reflective sublayer stacked sequentially, the first ultraviolet reflective sublayer being located between the Mth ultraviolet reflective sublayer and the emitting layer; M is an integer greater than or equal to 2.
31. The method for manufacturing an optical solar reflector according to claim 30, characterized in that, The steps for forming the m-th ultraviolet reflective sublayer include: The ultraviolet reflective layer sol solution was formed using the sol-gel method; The ultraviolet reflective layer sol solution is applied for the mth time on the side of the emitting layer opposite to the emitting substrate; The ultraviolet reflective layer sol solution on the emitting layer is subjected to the m-th curing treatment to form the m-th ultraviolet reflective sublayer; m is an integer greater than or equal to 1 and less than or equal to M.
32. The method for manufacturing an optical solar reflector according to claim 31, characterized in that, The process of applying the ultraviolet reflective layer sol solution to the side of the emitting layer opposite to the emitting substrate for the mth time includes dip coating, roller coating, or spin coating.
33. The method for manufacturing an optical solar reflector according to claim 32, characterized in that, The parameters of the immersion-lifting method include: the immersion speed in the ultraviolet reflective layer sol solution is 3000μm / s to 5000μm / s, the lifting speed is 1000μm / s to 3000μm / s, and the immersion time in the ultraviolet reflective layer sol solution is 1min to 3min.
34. The method for manufacturing an optical solar reflector according to claim 31, characterized in that, The temperatures of the first curing treatment to the (M-1)th curing treatment are all lower than the temperature of the Mth curing treatment; the times of the first curing treatment to the (M-1)th curing treatment are all lower than the times of the Mth curing treatment.
35. The method for manufacturing an optical solar reflector according to claim 34, characterized in that, The temperature difference between the Mth curing treatment and the jth curing treatment is 50℃~200℃; the time difference between the Mth curing treatment and the jth curing treatment is 30min~50min; j is an integer greater than or equal to 1 and less than or equal to M-1.
36. The method for manufacturing an optical solar reflector according to claim 35, characterized in that, During the formation of the j-th ultraviolet reflective sublayer, the temperature of the j-th curing treatment is 200℃~300℃, and the time of the j-th curing treatment is 20min~30min; During the formation of the Mth ultraviolet reflective sublayer, the temperature of the Mth curing treatment is 200℃~500℃, and the time of the Mth curing treatment is 50min~80min.
37. The method for manufacturing an optical solar reflector according to claim 31, characterized in that, The steps for forming the UV reflective layer sol solution using the sol-gel method include: The first ultraviolet reflective layer sol solution was formed using the sol-gel method; The second ultraviolet reflective layer sol solution was formed using the sol-gel method; After mixing the first ultraviolet reflective layer sol and the second ultraviolet reflective layer sol, the mixture is aged to form the ultraviolet reflective layer sol.
38. The method for manufacturing an optical solar reflector according to claim 37, characterized in that, The mass ratio of the first ultraviolet reflective layer sol to the second ultraviolet reflective layer sol is 2:1 to 5:1; The aging process takes 7 to 30 days.
39. The method for manufacturing an optical solar reflector according to claim 37, characterized in that, The steps for forming the first ultraviolet reflective layer sol solution using the sol-gel method include: Titanate, alcohol, organic acid and inorganic acid are mixed to form the first ultraviolet reflective layer sol solution; Alternatively, zinc-containing organic salts, alcohols, organic acids, and inorganic acids can be mixed to form the first ultraviolet reflective layer sol solution.
40. The method for manufacturing an optical solar reflector according to claim 39, characterized in that, The molar ratio of titanate to alcohol is 1:45 to 1:60; or, the molar ratio of zinc-containing organic salt to alcohol is 1:45 to 1:60; the molar ratio of hydrogen ions in organic and inorganic acids to alcohol is 1:60 to 4:60; the molar ratio of hydrogen ions in organic and inorganic acids to water is 4:0.4 to 4:0.
7.
41. The method for manufacturing an optical solar reflector according to claim 39, characterized in that, The titanate includes: tetraethyl titanate, tetraisopropyl titanate, or tetrabutyl titanate; The zinc-containing organic salts include: zinc acetate and zinc diethyldithiocarbamate; The alcohols include: methanol, ethanol, isopropanol, or butanol; The organic acids include: oxalic acid, acetic acid, or citric acid; The inorganic acids include hydrochloric acid, nitric acid, or sulfuric acid.
42. The method for manufacturing an optical solar reflector according to claim 37, characterized in that, The steps for forming the second ultraviolet reflective layer sol solution using the sol-gel method include: mixing rare earth salts, alcohols and chelating agents to form the second ultraviolet reflective layer sol solution.
43. The method for manufacturing an optical solar reflector according to claim 42, characterized in that, The molar ratio of rare earth salt to alcohol is 1:30 to 1:40; the molar ratio of alcohol to chelating agent is 40:0.5 to 40:
2.
44. The method for manufacturing an optical solar reflector according to claim 42, characterized in that, The rare earth salts include: carbonates, oxalates, or chlorides; The alcohols include: methanol, ethanol, isopropanol, or butanol; The chelating agent includes: polyacrylic acid, polymaleic anhydride, ethylenediaminetetraacetic acid, or acetylacetone.
45. The method for manufacturing an optical solar reflector according to claim 31, characterized in that, The ultraviolet reflective layer sol solution includes one or a combination of titanium sol solution, cerium sol solution, lanthanum sol solution, zinc sol solution, or yttrium sol solution.
46. The method for manufacturing an optical solar reflector according to claim 29, characterized in that, Also includes: A transparent conductive film is formed on the surface of the ultraviolet reflective layer facing away from the emitting layer.
47. The method for manufacturing an optical solar reflector according to claim 46, characterized in that, The method for forming the transparent conductive film includes magnetron sputtering or sol-gel process.
48. The method for manufacturing an optical solar reflector according to claim 16, characterized in that, Also includes: A metallic reflective layer is formed on the surface of the emitting substrate facing away from the emitting layer; A metal protective layer is formed on the surface of the metal reflective layer that faces away from the reflective layer.
Citation Information
Patent Citations
Composite radiation refrigeration film
CN110216924A
Anti-static ultra-low absorption solar spectrum reflector and preparation method thereof
CN112666644A
Radiative cooling device and method of manufacturing the same
US20210310700A1