Silicon negative electrode material and preparation method thereof
By composite Mg-P coating on the surface of silicon particles and then etching and heat treatment, the volume expansion problem of silicon anode materials was solved, the cycle stability and capacity were improved, and high-efficiency lithium-ion battery performance was achieved.
Patent Information
- Application Number
- CN202311683027.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Silicon anode materials in lithium-ion batteries suffer from structural collapse due to volume expansion and contraction, resulting in short cycle life and difficulty in forming a stable solid electrolyte interface film, which affects battery performance.
A Mg-P coating was composited on the surface of silicon particles using vapor deposition, and the adhesion was improved by etching and heat treatment to form Mg-P/Si particles.
It improves the cycle stability and capacity of silicon anode materials, maintaining a high capacity of 1730 mAh/g after 150 cycles, significantly improving cycle performance.
Smart Images

Figure CN117673305B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery materials technology, specifically to a silicon anode material and its preparation method. Background Technology
[0002] Lithium-ion batteries are used not only in power batteries but also play a crucial role in energy storage. The future demands for the energy density of lithium-ion batteries are increasingly higher. As a next-generation anode material, silicon (Si) has a theoretical capacity 10 times higher than graphite, thus attracting significant attention. However, because silicon is a semiconductor material with low conductivity, the Si-Li alloying and dealloying processes during electrochemical charging and discharging, along with the insertion and extraction of lithium ions, cause the material's volume to expand and contract by more than 300%. The resulting mechanical forces gradually pulverize the material, causing structural collapse and ultimately leading to the detachment of the electrode active material from the current collector, resulting in loss of electrical contact and a significant reduction in battery cycle performance. Furthermore, due to this volume effect, silicon struggles to form a stable solid electrolyte interphase (SEI) film in the electrolyte. With the destruction of the electrode structure, new SEI films continuously form on the exposed silicon surface, exacerbating silicon corrosion and capacity decay. Therefore, the cycle life of Si anodes needs further improvement.
[0003] Compounds of Si with other elements can effectively improve cycle life, but studies have found that they significantly reduce actual capacity. Therefore, in order to effectively utilize the high potential capacity of Si anodes, it is necessary to find ways to compensate for its lifespan shortcomings while adhering to elemental Si as the active material. Summary of the Invention
[0004] To address the technical problems of short cycle life, unstable cycling, and low actual capacity of Si anodes, this invention provides a silicon anode material and its preparation method, which can still achieve a high capacity of 1730 mAh / g even after 150 cycles.
[0005] In a first aspect, the present invention provides a method for preparing a silicon anode material, comprising the following steps: SiO2 particles are etched to obtain etched SiO2 particles; a mixed phase Mg-P is synthesized on the surface of the etched SiO2 particles by vapor deposition to form Mg-P / Si particles; and the Mg-P / Si particles are then heat-treated to obtain the silicon anode material.
[0006] Furthermore, this includes the following steps: (1) Add SiO2 particles to hydrofluoric acid solution and stir to obtain etched SiO2 particles; (2) In a glove box filled with argon, the etched SiO2 particles and Mg powder with a molar ratio of 1:2.5-7.5 are placed in an alumina ceramic boat, and then the alumina ceramic boat is placed in a steel cylinder. After the steel cylinder is sealed, the etched SiO2 particles and Mg powder are in an argon protective atmosphere. (3) Place the sealed steel cylinder in a tube furnace, heat it to 680-700℃, and keep it under vacuum for 30-60 minutes; (4) The product obtained in step (3) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750-770°C in flowing N2. The reaction is maintained for 1-2 hours. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture for 0.5-1 hours. (5) Heat-treat the product obtained in step (4) under an argon atmosphere to obtain the final product.
[0007] Furthermore, the concentration of the hydrofluoric acid solution in step (1) is 0.1M.
[0008] Furthermore, in step (2), the molar ratio of the etched SiO2 particles to Mg powder is 1:5.0.
[0009] Furthermore, in step (3), the temperature is increased to 685°C at a heating rate of 10°C / min and maintained under vacuum for 45 minutes.
[0010] Furthermore, in step (4), the flow rate of N2 is 10 mL / min, and the reaction is maintained for 1 hour after heating to 750 °C.
[0011] Furthermore, in step (4), the molar concentration of oxygen in the O2 / N2 mixture is 1.0%, the flow rate of the mixture is 20 mL / min, and the product is passivated in the O2 / N2 mixture for 0.5 hours.
[0012] Furthermore, in step (5), the heat treatment temperature is 700-800℃ and the time is 1 hour.
[0013] Secondly, the present invention provides a silicon anode material prepared by the above-described preparation method.
[0014] The beneficial effects of this invention are as follows: This invention provides a silicon anode material that overcomes the shortcomings of pure Si by combining Si particles with Mg-P materials. By employing vapor deposition to composite a Mg-P coating into Si particles, and through surface etching for roughening and heat treatment, the adhesion between the Mg-P coating and Si particles is improved, thereby enhancing the cycle stability of the Si anode material. After 150 cycles, it still maintains a high capacity of 1730 mAh / g, significantly superior to pure Si anodes. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 These are the charge-discharge curves for the first cycle of the examples and comparative examples.
[0017] Figure 2 This is a comparison graph of cycle life between the examples and the comparative examples. Detailed Implementation
[0018] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.
[0019] Example 1 (1) Add SiO2 particles to 0.1M hydrofluoric acid solution and stir for 1 hour to roughen the surface and obtain etched SiO2 particles; (2) In a glove box filled with argon, the etched SiO2 particles and Mg powder (40 mesh) with a molar ratio of 1:5.0 are placed in an alumina ceramic boat, and then the alumina ceramic boat is placed in a steel cylinder. After the steel cylinder is sealed, the etched SiO2 particles and Mg powder are in an argon protective atmosphere. (3) Place the sealed steel cylinder in a tube furnace and heat it to 685°C at a heating rate of 10°C / min, and maintain the temperature at 685°C under vacuum for 45 minutes; (4) The product obtained in step (3) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750°C in flowing N2. The flow rate of N2 is 10 mL / min. The reaction is maintained at 750°C for 1 hour. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture with an O2 molar concentration of 1.0 mol% for 0.5 hours. The flow rate of the O2 / N2 mixture is 20 mL / min. (5) The product obtained in step (4) is treated in an argon atmosphere at 800°C for 1 hour to obtain the final product.
[0020] Comparative Example 1 (1) In a glove box filled with argon, SiO2 particles and Mg powder (40 mesh) with a molar ratio of 1:5.0 were placed in an alumina ceramic boat, and then the alumina ceramic boat was placed in a steel cylinder. After the steel cylinder was sealed, the SiO2 particles and Mg powder were in an argon protective atmosphere. (2) Place the sealed steel cylinder in a tube furnace and heat it to 685°C at a heating rate of 10°C / min, and maintain the temperature at 685°C under vacuum for 45 minutes; (3) The product obtained in step (2) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750°C in flowing N2. The flow rate of N2 is 10 mL / min. The reaction is maintained at 750°C for 1 hour. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture with an O2 molar concentration of 1.0 mol% for 0.5 hours to obtain the final product. The flow rate of the O2 / N2 mixture is 20 mL / min.
[0021] Comparative Example 2 (1) Add SiO2 particles to 0.1M hydrofluoric acid solution and stir for 1 hour to roughen the surface and obtain etched SiO2 particles; (2) In a glove box filled with argon, the etched SiO2 particles and Mg powder (40 mesh) with a molar ratio of 1:5.0 are placed in an alumina ceramic boat, and then the alumina ceramic boat is placed in a steel cylinder. After the steel cylinder is sealed, the etched SiO2 particles and Mg powder are in an argon protective atmosphere. (3) Place the sealed steel cylinder in a tube furnace and heat it to 685°C at a heating rate of 10°C / min, and maintain the temperature at 685°C under vacuum for 45 minutes; (4) The product obtained in step (3) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750°C in flowing N2. The flow rate of N2 is 10 mL / min. The reaction is maintained at 750°C for 1 hour. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture with an O2 molar concentration of 1.0 mol% for 0.5 hours to obtain the final product. The flow rate of the O2 / N2 mixture is 20 mL / min. Comparative Example 3 (1) In a glove box filled with argon, SiO2 particles and Mg powder (40 mesh) with a molar ratio of 1:5.0 were placed in an alumina ceramic boat, and then the alumina ceramic boat was placed in a steel cylinder. After the steel cylinder was sealed, the SiO2 particles and Mg powder were in an argon protective atmosphere. (2) Place the sealed steel cylinder in a tube furnace and heat it to 685°C at a heating rate of 10°C / min, and maintain the temperature at 685°C under vacuum for 45 minutes; (3) The product obtained in step (2) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750°C in flowing N2. The flow rate of N2 is 10 mL / min. The reaction is maintained at 750°C for 1 hour. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture with an O2 molar concentration of 1.0 mol% for 0.5 hours. The flow rate of the O2 / N2 mixture is 20 mL / min. (4) The product obtained in step (3) is treated in an argon atmosphere at 800°C for 1 hour to obtain the final product.
[0022] Comparative Example 4 Untreated Si particles.
[0023] Battery test: Electrodes were prepared using the final product of Example 1, the final products of Comparative Examples 1-3, and the untreated Si particles of Comparative Example 4, respectively, as test negative electrodes. Li foil was used as the counter electrode, and 1M LiTFSA / 1-methyl-1-propylpyrrolidineonium bis(fluorosulfonyl)imide (Py13-FSA) was used as the electrolyte.
[0024] The charge / discharge conditions are set to a potential width of 0.005-2.000V vs. Li / Li. + The experiment was conducted under conditions of a current density of 1.4 A / g (0.4 C).
[0025] from Figure 1 The charge-discharge curves show that potential plateaus due to Si and Li alloying and dealloying are observed near 0.1V on the charging side and 0.4V on the discharging side in all materials. Although Mg does not exhibit Li insertion / extraction activity, the composite electrode still shows a reversible Li storage-release reaction, thus Mg-P possesses certain Li activity.
[0026] from Figure 2It can be seen that Comparative Example 4 experienced rapid capacity decay due to the significant volume change. The Si anodes from different embodiments showed varying degrees of improvement in cycle life. Comparative Example 1 not only improved the mechanical properties of the Si active material but also increased electronic conductivity by approximately 80 times. Comparative Example 3 further improved cycle performance, maintaining a capacity of 1350 mAh / g after 150 charge-discharge cycles. While Comparative Example 2 showed some capacity improvement, its cycle decay behavior was similar to that of the untreated Si anode. Example 1 demonstrated significantly improved cycle stability, maintaining a high capacity of 1730 mAh / g even after 150 cycles, indicating that volume collapse of the active material was greatly prevented. Based on these results, it is speculated that electrolytic deposition of Mg-P solely on the Si surface does not improve adhesion; however, after heat treatment, Mg diffuses to the rough Si surface and anchors, significantly improving adhesion.
[0027] Although the present invention has been described in detail with reference to the accompanying drawings and preferred embodiments, the present invention is not limited thereto. Various equivalent modifications or substitutions can be made to the embodiments of the present invention by those skilled in the art without departing from the spirit and essence of the invention, and such modifications or substitutions should all be within the scope of the present invention. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should also be covered within the protection scope of the present invention.
Claims
1. A method for preparing a silicon anode material, characterized in that, The process includes the following steps: SiO2 particles are etched to obtain etched SiO2 particles; a mixed phase Mg-P is synthesized on the surface of the etched SiO2 particles using a vapor deposition method to form Mg-P / Si particles; and the Mg-P / Si particles are then heat-treated to obtain silicon anode material.
2. The method for preparing the silicon anode material as described in claim 1, characterized in that, Includes the following steps: (1) Add SiO2 particles to hydrofluoric acid solution and stir to obtain etched SiO2 particles; (2) In a glove box filled with argon, the etched SiO2 particles and Mg powder with a molar ratio of 1:2.5-7.5 are placed in an alumina ceramic boat, and then the alumina ceramic boat is placed in a steel cylinder. After the steel cylinder is sealed, the etched SiO2 particles and Mg powder are in an argon protective atmosphere. (3) Place the sealed steel cylinder in a tube furnace, heat it to 680-700℃, and keep it under vacuum for 30-60 minutes; (4) The product obtained in step (3) is loaded into a quartz boat and placed on one side of a quartz tube, and sodium hypophosphite is placed on the other side of the quartz tube. Then the quartz tube is placed in a tube furnace and heated to 750-770°C in flowing N2. The reaction is maintained for 1-2 hours. After that, the product is cooled to room temperature and passivated in an O2 / N2 mixture for 0.5-1 hours. (5) Heat-treat the product obtained in step (4) under an argon atmosphere to obtain the final product.
3. The method for preparing the silicon anode material as described in claim 2, characterized in that, The concentration of the hydrofluoric acid solution in step (1) is 0.1M.
4. The method for preparing the silicon anode material as described in claim 2, characterized in that, In step (2), the molar ratio of SiO2 particles and Mg powder etched is 1:5.
0.
5. The method for preparing the silicon anode material as described in claim 2, characterized in that, In step (3), the temperature is increased to 685°C at a heating rate of 10°C / min and held under vacuum for 45 minutes.
6. The method for preparing the silicon anode material as described in claim 2, characterized in that, In step (4), the flow rate of N2 is 10 mL / min, and the reaction is maintained for 1 hour after heating to 750 °C.
7. The method for preparing the silicon anode material as described in claim 2, characterized in that, In step (4), the molar concentration of oxygen in the O2 / N2 mixture is 1.0%, the flow rate of the mixture is 20 mL / min, and the product is passivated in the O2 / N2 mixture for 0.5 hours.
8. The method for preparing the silicon anode material as described in claim 2, characterized in that, In step (5), the heat treatment temperature is 700-800℃ and the time is 1 hour.
9. A silicon anode material prepared by the method for preparing silicon anode material according to any one of claims 1-8.
Citation Information
Patent Citations
Fluorine-free preparation method for three-dimensional porous silica powder anode material of lithium ion battery
CN102237519A
Negative electrode material for secondary battery, and its manufacturing method
JP2010170943A