A high specific capacity oxygen / sulfur co-doped porous carbon negative electrode material, a preparation method and application thereof

By using an oxygen/sulfur co-doped porous carbon anode material preparation method, the problems of low heteroatom content at the edge of carbon anode materials and complicated preparation process have been solved, achieving high sodium storage capacity and excellent electrochemical performance, which is suitable for industrial production.

CN117673325BActive Publication Date: 2026-11-20ZHENGZHOU ZHONGKE EMERGING IND TECH RES INST +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311835969.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2026-11-20
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Existing carbon anode materials have low edge heteroatom content and complicated preparation processes, resulting in poor sodium storage capacity and kinetic performance of sodium-ion batteries, and are not conducive to low-cost industrial production.

Method used

A method for preparing oxygen/sulfur co-doped porous carbon anode materials is adopted. The oxygen/sulfur co-doping polymerization reaction is carried out in a reactor with a mixture of oxygen and nitrogen gas under thermal stirring. Combined with micron-scale molten salt template and high-temperature carbonization treatment, a porous framework carbon nanosheet material is prepared, achieving high edge heteroatom content and ultrathin carbon nanosheet structure.

Benefits of technology

This method improves the sodium storage capacity and kinetic performance of sodium-ion battery anode materials, while simplifying the preparation process and making it suitable for industrial production. The porous and disordered microcrystalline structure on the material surface provides more active sites for sodium storage. The initial discharge specific capacity can reach 920-1200 mAh/g, and it still maintains 280-600 mAh/g after 100 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117673325B_ABST
    Figure CN117673325B_ABST
Patent Text Reader

Abstract

The application discloses a high-specific-capacity oxygen / sulfur co-doped porous carbon negative material and a preparation method and application thereof, and the preparation method is as follows: putting pitch and a sulfur aid into a reaction kettle, filling mixed gas of oxygen and nitrogen with a certain pressure, and then performing a heat stirring oxygen / sulfur co-doping polymerization reaction to obtain modified polymerized pitch; after grinding and mixing the modified polymerized pitch and a microscale fused salt template, performing carbonization treatment under nitrogen protection, washing with deionized water after cooling, and performing filtration and vacuum drying, a high-specific-capacity oxygen / sulfur co-doped porous carbon negative material for a sodium ion battery is obtained; the prepared oxygen / sulfur co-doped carbon negative material has a honeycomb-shaped porous frame composed of ultrathin carbon nanosheets and a relatively high edge heteroatom doping content; and the preparation method has a simple process flow and exhibits high specific capacity, excellent rate and cycle performance for a sodium ion battery negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon anode materials for sodium-ion batteries, specifically to a high-specific-capacity oxygen / sulfur co-doped porous carbon anode material, its preparation method, and its application. Background Technology

[0002] Sodium is abundant and widely distributed in the Earth's crust, making sodium-ion batteries a more attractive and promising energy storage technology. However, graphite, a commercially available anode material for lithium-ion batteries, is unsuitable for sodium-ion batteries. Therefore, designing high-performance anode materials is crucial for the practical application of sodium-ion batteries.

[0003] Among carbon materials, soft carbon possesses a large number of relatively ordered sps. 2 Carbon clusters and amorphous molecular structures, with their relatively easily tunable carbon microcrystalline structures, offer advantages in improving electronic conductivity and Na+. + The migration of these molecules allows for the achievement of ideal rate capability and cycling performance. As is well known, coal tar pitch is a typical soft carbon precursor, consisting of aromatic nuclei (relatively stable conjugated SPs). 2 Carbon) and side chains (peripheral SP) 3 Carbon-based anode materials have the advantages of low cost and high carbon yield. However, due to their high aromaticity and high degree of condensation, dense aromatic compounds undergo strong π-π interactions during carbonization, leading to severe rearrangement of planar molecules and the formation of tightly packed carbon layers. This is detrimental to the preparation of high-value-added, high-performance carbon anode materials for sodium-ion batteries. Therefore, improving the electrochemical performance of pitch-based carbon materials by adjusting their microstructure is a major challenge in achieving high-performance sodium-ion battery anode materials.

[0004] Invention patent CN115893373A converts low-cost polycyclic aromatic hydrocarbon products such as pitch and needle coke from the coal chemical industry into high-value-added carbon anode materials for sodium-ion batteries. To avoid graphitization of pitch and other polycyclic aromatic hydrocarbons during heat treatment, coal pitch is modified with fluorides to obtain a coal pitch-based anode carbon material for sodium-ion batteries with low graphitization. This anode carbon material exhibits an ultra-high sodium storage specific capacity of 450 mAh / g at a current density of 0.05 A / g, while also possessing good cycle life and rate performance. Invention patent CN117125694A The invention discloses a method for obtaining pitch-based carbon materials by high-temperature carbonization of pre-oxidized pitch with an alkaline activator. The oxidation inhibits the structural rearrangement of pitch during subsequent reactions, thereby forming disordered graphite microcrystals. The alkaline activator then etches the graphite microcrystals to obtain nanoscale microporous carbon materials. The resulting carbon materials, when used as the negative electrode of sodium-ion batteries, can significantly improve the sodium storage capacity and rate performance of the batteries. Patent CN116462182A discloses the preparation of nitrogen-sulfur dual-doped carbon materials and their application in sodium-ion batteries. This method increases the structural defects of pitch-based carbon materials, providing more active sites and thus improving their sodium storage performance.

[0005] Designing a well-designed edge defect structure through heteroatom modification can effectively improve the sodium storage capacity of soft carbon anodes. However, due to the difficulty in precisely customizing effective edge doping strategies based on molecular control, limited edge heteroatom doping often leads to low sodium storage capacity and slow kinetics. Furthermore, most heteroatom doping processes are cumbersome, hindering low-cost industrial production. Therefore, designing a preparation method with high edge heteroatom doping content and a simple fabrication process is of practical significance for sodium-ion battery anode materials. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies. In order to solve the problems of low edge heteroatom content and complicated preparation process of carbon anode materials, this invention provides a preparation method and application of high specific capacity oxygen / sulfur co-doped porous carbon anode materials, which can effectively solve the problem of low edge heteroatom content of carbon anode materials, thereby improving the sodium storage capacity of carbon anode materials, while also greatly simplifying the preparation process.

[0007] To achieve the above objectives, the technical solution of the present invention is implemented as follows: A method for preparing a high-specific-capacity oxygen / sulfur co-doped porous carbon anode material includes the following steps: (1) Add asphalt and sulfur additives to the reactor and fill it with a mixture of oxygen and nitrogen gas to carry out a hot-stirred oxygen / sulfur co-doping polymerization reaction to obtain modified polymerized asphalt; (2) The modified polymeric asphalt obtained in step (1) and the micron-sized molten salt template are ball-milled and mixed evenly to obtain a solid mixture. Under a nitrogen atmosphere, the solid mixture is placed in a tube furnace for high-temperature carbonization treatment. After cooling, it is washed with deionized water, filtered, and vacuum dried to obtain a high specific capacity oxygen / sulfur co-doped porous carbon anode material.

[0008] Furthermore, the asphalt in step (1) is any one or more of medium-low temperature coal tar pitch, high temperature coal tar pitch, petroleum asphalt, and coal liquefaction asphalt.

[0009] Furthermore, the sulfur additive in step (1) is any one or more of sublimed sulfur, thiourea, and ammonium sulfate.

[0010] Furthermore, in step (1), the mass ratio of asphalt to sulfur additive is 1:(0.1-5); the volume ratio of oxygen to nitrogen is 1:(1-5); and the initial pressure of the oxygen and nitrogen mixture is 0.1-2 MPa.

[0011] Furthermore, in step (1), the polymerization reaction temperature is 150-220℃, the time is 1-5h, and the stirring rate is 100-300r / min.

[0012] Furthermore, in step (2), the mass ratio of modified polymeric asphalt to micron-sized molten salt template is 1:(10-20); the ball milling speed is 100-300 r / min, and the time is 2-4 h; the carbonization temperature is 600-800℃, and the time is 1-4 h.

[0013] Furthermore, the micron-sized molten salt template in step (2) is a mixed salt of sodium chloride and potassium chloride with a mass ratio of 1:(0-1), and an average particle size of 5-8 μm. The melting temperature is controlled by the ratio of molten salt.

[0014] Furthermore, the micron-sized molten salt template is prepared by recrystallization, which includes the following steps: gradually adding a prepared supersaturated mixed salt solution to anhydrous ethanol, stirring to precipitate white crystals, filtering and drying to obtain the micron-sized molten salt template. Recrystallization is an effective technique that can control the size of crystal particles and improve the uniformity of the template, thereby effectively influencing the morphology of the evolved 3D material.

[0015] Furthermore, the high specific capacity oxygen / sulfur co-doped porous carbon anode material prepared according to the above method has a porous framework structure, which is composed of a large number of ultrathin carbon nanosheets, exhibiting a regular honeycomb three-dimensional morphology; the oxygen / sulfur heteroatom content at the edge of the carbon nanosheet (i.e. the surface of the nanosheet) is 10-20 at.%.

[0016] Furthermore, high-capacity oxygen / sulfur co-doped porous carbon anode materials are applied in sodium-ion batteries or lithium-ion batteries.

[0017] The present invention has the following beneficial effects: (1) The present invention obtains oxygen / sulfur modified polymeric asphalt through oxygen / sulfur co-doping polymerization reaction, then ball mills the modified polymeric asphalt with the assistance of molten salt template, and then carbonizes it at high temperature in a tube furnace. This one-step in-situ thermal synthesis method achieves a high content of edge heteroatoms and an ultrathin carbon nanosheet structure.

[0018] (2) The oxygen / sulfur-doped honeycomb porous carbon anode material prepared by this invention has a porous framework structure composed of three-dimensional honeycomb ultrathin carbon nanosheets. The porous, defective, and disordered microcrystalline structure on the surface of the material provides adsorption and sodium storage active sites for the asphalt material. At the same time, compared with the porous carbon nanosheets of ordinary pure asphalt, the heteroatom content at the edge (surface of the nanosheet) of the carbon nanosheets prepared by this method is 10 at.%-20 at.%, with oxygen existing in the form of carbonyl groups and sulfur in the form of oxidized sulfur (C-SO4). x -C) and thiophene-type sulfur (CSC 2p) 3 / 2 and CSC 2p 1 / 2 The presence of sodium in the form of edge heteroatoms improves sodium storage capacity and sodium ion dynamics.

[0019] (3) The oxygen / sulfur co-doped honeycomb porous carbon anode material of the present invention has excellent electrochemical properties as a sodium-ion battery anode material. At a current density of 0.1 A / g, the initial discharge specific capacity is 920-1200 mAh / g, and the reversible discharge specific capacity can be maintained at 280-600 mAh / g after 100 cycles.

[0020] (4) In the prior art, most heteroatom doping processes are cumbersome, generally requiring oxidative cross-linking first, followed by sulfur doping, which is not conducive to low-cost industrial production. The preparation process of the porous carbon nanosheets obtained in this invention is carried out in a reactor under a closed gas atmosphere, which can easily achieve oxygen cross-linking while doing sulfur doping, which is conducive to low-cost industrial production. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1This is a SEM image of the oxygen / sulfur co-doped porous carbon anode material of Embodiment 1 of the present invention.

[0023] Figure 2 This is the XPS image of the oxygen / sulfur co-doped porous carbon anode material in Example 1 of the present invention (SOCN3 is the oxygen / sulfur co-doped porous carbon anode material, and CN is the undoped porous carbon anode material in Comparative Example 1).

[0024] Figure 3 This is a constant current charge / discharge curve of the oxygen / sulfur co-doped porous carbon anode material in Embodiment 1 of the present invention; SOCN3 is the oxygen / sulfur co-doped porous carbon anode material, and 1st, 3rd, and 5th are the first charge / discharge, third charge / discharge, and fifth charge / discharge curves, respectively.

[0025] Figure 4 The diagram shows the cycle performance of the porous carbon anode material; SOCN3 is the oxygen / sulfur co-doped porous carbon anode material of Example 1 of this invention, and CN is the undoped porous carbon anode material of Comparative Example 1. Detailed Implementation

[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] Example 1 This embodiment provides a high-specific-capacity oxygen / sulfur co-doped porous carbon anode material, and the specific preparation steps are as follows: 1.5g of medium-low temperature coal tar pitch and 4.5g of sublimed sulfur were placed in a 50mL reactor at a mass ratio of 1:3. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 0.1 MPa. The volume ratio of oxygen to nitrogen was 1:4. The polymerization reaction was carried out at 180℃ for 3 hours with a stirring rate of 150 r / min to obtain modified polymerized pitch.

[0028] Micron-sized sodium chloride templates were obtained by recrystallization. A supersaturated sodium chloride solution was prepared, and then the supersaturated sodium chloride solution was added dropwise to anhydrous ethanol. The mixture was stirred to precipitate white crystals, which were then filtered and dried to obtain a molten salt template with a particle size of 8 μm.

[0029] 0.5 g of modified polymeric asphalt was ball-milled with 5 g of molten salt template with an average particle size of 8 μm for 4 h at a rotation speed of 300 rpm. Then, it was carbonized at 600 °C under a nitrogen atmosphere for 2 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain sulfur / oxygen-doped porous carbon anode material.

[0030] The morphology of the obtained sulfur / oxygen-doped porous carbon anode material is as follows: Figure 1 As shown, the obtained negative electrode material has a porous framework structure, which is composed of a large number of ultrathin carbon nanosheets and exhibits a regular honeycomb three-dimensional morphology.

[0031] XPS analysis of the obtained oxygen / sulfur co-doped porous carbon anode material is as follows: Figure 2 As shown, SOCN3 is an oxygen / sulfur co-doped porous carbon anode material, in which oxygen exists in the form of carbonyl groups, while sulfur exists in the form of oxidized sulfur (C-SO4). x -C) and thiophene-type sulfur (CSC 2p) 3 / 2 and CSC 2p 1 / 2 It exists in the form of ). Among them, the oxygen content is 7.66 at.%, and the sulfur content is 10.61 at.%.

[0032] It was used as the negative electrode material to assemble a sodium-ion half-cell and its electrochemical performance was tested.

[0033] The preparation process and electrochemical performance of the electrode sheet in this embodiment are as follows: Weigh appropriate amounts of negative electrode material, polyvinylidene fluoride, and acetylene black, along with an appropriate amount of N-methylpyrrolidone, at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 hours, the mixture is uniformly coated with copper foil and vacuum dried at 80℃ for 24 hours to obtain the battery electrode. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, a sodium-ion button cell is assembled in a glove box. After assembly, the cell is allowed to stand for 12 hours, and its electrochemical performance is measured under the following conditions: current density 0.1 A / g.

[0034] The first charge-discharge curve of a sodium-ion half-cell assembled with the obtained oxygen / sulfur co-doped porous carbon anode material as the anode is shown in the figure. Figure 3 As shown, in this embodiment, oxygen / sulfur co-doped porous carbon exhibits both plateau capacity and slope region capacity when used as the anode material for sodium-ion half-cells. Furthermore, it has a very high initial discharge specific capacity, reaching 1100 mAh / g, and a charge specific capacity of 700 mAh / g.

[0035] The cycle performance of sodium-ion half-cells with oxygen / sulfur co-doped porous carbon as the negative electrode material is as follows: Figure 4As shown, the initial discharge specific capacity is 1100 mAh / g, and after 5 charge-discharge cycles, the discharge specific capacity stabilizes at around 600 mAh / g. After 100 cycles, the discharge specific capacity can still reach 580 mAh / g.

[0036] Example 2 This embodiment provides a high specific capacity oxygen / sulfur co-doped porous carbon anode material, and the preparation steps are as follows: 1.5 g of medium-low temperature coal tar pitch and 0.15 g of thiourea were placed in a 50 mL reactor at a mass ratio of 1:0.1. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 0.1 MPa. The volume ratio of oxygen to nitrogen was 1:5. The polymerization reaction was carried out at 150 °C for 5 h with a stirring rate of 100 r / min to obtain modified polymerized asphalt.

[0037] Micron-sized mixed molten salt templates of sodium chloride and potassium chloride were obtained by recrystallization. A supersaturated sodium chloride and potassium chloride mixed solution was prepared at a mass ratio of 1:0.1. Then, the supersaturated solution was added dropwise to anhydrous ethanol, and white crystals were precipitated by stirring. After filtration and drying, molten salt templates with a particle size of 8 μm were obtained.

[0038] 0.5 g of modified polymeric asphalt was ball-milled with 5 g of molten salt template with an average particle size of 8 μm for 4 h at a speed of 100 rpm, and then carbonized at 600 ℃ under a nitrogen atmosphere for 4 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain a sulfur / oxygen-doped porous carbon anode material with an oxygen content of 8.35 at.% and a sulfur content of 2.4 at.%. This material was used as the anode material to assemble sodium-ion half-cells, and its electrochemical performance was tested.

[0039] The preparation process of the electrode sheet in this embodiment is as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0040] The electrochemical performance of the electrode sheet in this embodiment is as follows: The initial discharge specific capacity is 920 mAh / g at a current density of 0.1 A / g, and the discharge specific capacity can still reach 280 mAh / g after 100 cycles.

[0041] Example 3 The preparation steps of a high specific capacity oxygen / sulfur co-doped porous carbon anode material are as follows: 1.5g of petroleum asphalt and 7.5g of sublimed sulfur were placed in a 50mL reactor at a mass ratio of 1:5. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 1 MPa. The volume ratio of oxygen to nitrogen was 1:1. The polymerization reaction was carried out at 220℃ for 1 hour with a stirring rate of 300r / min to obtain modified polymerized asphalt.

[0042] Micron-sized mixed molten salt templates of sodium chloride and potassium chloride were obtained by recrystallization. A supersaturated sodium chloride and potassium chloride mixed solution was prepared at a mass ratio of 1:1. Then, the supersaturated sodium chloride and potassium chloride mixed solution was added dropwise to anhydrous ethanol. The mixture was stirred to precipitate white crystals. After filtration and drying, a molten salt template with an average particle size of 5 μm was obtained.

[0043] 0.5 g of modified polymeric asphalt was ball-milled with 10 g of molten salt template with an average particle size of 5 μm for 4 h at a speed of 300 rpm, and then carbonized at 800 ℃ under a nitrogen atmosphere for 1 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain a sulfur / oxygen-doped porous carbon anode material with an oxygen content of 7.88 at.% and a sulfur content of 10.22 at.%. This material was used as the anode material to assemble sodium-ion half-cells, and its electrochemical performance was tested.

[0044] The preparation process of the electrode sheet in this embodiment is as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0045] The electrochemical performance of the electrode sheet in this embodiment is as follows: The initial discharge specific capacity is 1200 mAh / g at a current density of 0.1 A / g, and the discharge specific capacity can still reach 587 mAh / g after 100 cycles.

[0046] Example 4 This embodiment provides a high specific capacity oxygen / sulfur co-doped porous carbon anode material, and the preparation steps are as follows: 1.5g of high-temperature coal tar pitch and 7.5g of ammonium sulfate were placed in a 50mL reactor at a mass ratio of 1:5. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 2 MPa. The volume ratio of oxygen to nitrogen was 1:4. The polymerization reaction was carried out at 180℃ for 3 hours with a stirring rate of 150r / min to obtain modified polymerized asphalt.

[0047] Micron-sized mixed molten salt templates of sodium chloride and potassium chloride were obtained by recrystallization. A supersaturated sodium chloride and potassium chloride mixed solution was prepared at a mass ratio of 1:0.2. Then, the supersaturated sodium chloride solution was added dropwise to anhydrous ethanol, and white crystals were precipitated by stirring. After filtration and drying, molten salt templates with an average particle size of 7 μm were obtained.

[0048] 0.5 g of modified polymeric asphalt was ball-milled with 10 g of molten salt template with an average particle size of 7 μm for 2 h at a speed of 300 rpm, and then carbonized at 800 ℃ under a nitrogen atmosphere for 2 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain a sulfur / oxygen-doped porous carbon anode material with an oxygen content of 8.11 at.% and a sulfur content of 4.12 at.%. This material was used as the anode material to assemble sodium-ion half-cells, and its electrochemical performance was tested.

[0049] The preparation process of the electrode sheet in this embodiment is as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0050] The electrochemical performance of the electrode sheet in this embodiment is as follows: The initial discharge specific capacity is 960 mAh / g at a current density of 0.1 A / g, and the discharge specific capacity can still reach 380 mAh / g after 100 cycles.

[0051] Example 5 This embodiment provides a high specific capacity oxygen / sulfur co-doped porous carbon anode material, and the preparation steps are as follows: 2g of petroleum asphalt and 4g of ammonium sulfate were placed in a 50mL reactor at a mass ratio of 1:2. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 1 MPa. The volume ratio of oxygen to nitrogen was 1:2. The polymerization reaction was carried out at 200℃ for 1.5h with a stirring rate of 240r / min to obtain modified polymerized asphalt.

[0052] Micron-sized mixed molten salt templates of sodium chloride and potassium chloride were obtained by recrystallization. A supersaturated sodium chloride and potassium chloride mixed solution was prepared at a mass ratio of 1:0.8. Then, the supersaturated sodium chloride solution was added dropwise to anhydrous ethanol, and white crystals were precipitated by stirring. After filtration and drying, molten salt templates with an average particle size of 5 μm were obtained.

[0053] 1.0 g of modified polymeric asphalt was ball-milled with 15 g of molten salt template with an average particle size of 5 μm for 4 h at a speed of 200 rpm, and then carbonized at 780 ℃ under a nitrogen atmosphere for 2 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain a sulfur / oxygen-doped porous carbon anode material with an oxygen content of 7.13 at.% and a sulfur content of 2.86 at.%. This material was used as the anode material to assemble sodium-ion half-cells, and its electrochemical performance was tested.

[0054] The preparation process of the electrode sheet in this embodiment is as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0055] The electrochemical performance of the electrode sheet in this embodiment is as follows: The initial discharge specific capacity is 940 mAh / g at a current density of 0.1 A / g, and the discharge specific capacity can still reach 330 mAh / g after 100 cycles.

[0056] Example 6 This embodiment provides a high specific capacity oxygen / sulfur co-doped porous carbon anode material, and the preparation steps are as follows: 1.5g of high-temperature coal tar pitch and 6g of ammonium sulfate were placed in a 50mL reactor at a mass ratio of 1:4. A mixture of oxygen and nitrogen was introduced into the reactor to make the initial pressure about 0.5 MPa. The volume ratio of oxygen to nitrogen was 1:3. The polymerization reaction was carried out at 160℃ for 3 hours with a stirring rate of 220r / min to obtain modified polymerized asphalt.

[0057] Micron-sized mixed molten salt templates of sodium chloride and potassium chloride were obtained by recrystallization. A supersaturated sodium chloride and potassium chloride mixed solution was prepared at a mass ratio of 1:0.5. Then, the supersaturated sodium chloride solution was added dropwise to anhydrous ethanol, and white crystals were precipitated by stirring. After filtration and drying, molten salt templates with an average particle size of 6 μm were obtained.

[0058] 1.0 g of modified polymeric asphalt was ball-milled with 12 g of molten salt template with an average particle size of 6 μm for 2.5 h at a speed of 200 rpm, and then carbonized at 650 ℃ under a nitrogen atmosphere for 2.5 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water, and dried to obtain a sulfur / oxygen-doped porous carbon anode material with an oxygen content of 7.22 at.% and a sulfur content of 3.11 at.%. This material was used as the anode material to assemble sodium-ion half-cells, and its electrochemical performance was tested.

[0059] The preparation process of the electrode sheet in this embodiment is as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0060] The electrochemical performance of the electrode sheet in this embodiment is as follows: The initial discharge specific capacity is 950 mAh / g at a current density of 0.1 A / g, and the discharge specific capacity can still reach 360 mAh / g after 100 cycles.

[0061] Comparative Example 1: This comparative example provides an undoped porous carbon anode material. The preparation steps differ from those in Example 1 in that it does not undergo hetero (oxygen-sulfur) atom doping; the remaining steps are the same. The specific steps are as follows: Micron-sized sodium chloride templates were obtained by recrystallization. A supersaturated sodium chloride solution was prepared, and then the supersaturated sodium chloride solution was added dropwise to anhydrous ethanol. The mixture was stirred to precipitate white crystals, which were then filtered and dried to obtain a micron-sized sodium chloride template.

[0062] 0.5 g of asphalt was ball-milled with 5 g of micron-sized NaCl template for 4 h at 300 rpm, and then carbonized at 600 ℃ under a nitrogen atmosphere for 2 h at a nitrogen flow rate of 300 mL / min. After carbonization, the sample was allowed to cool naturally, washed with water and dried to obtain undoped porous carbon anode material. This material was used as the anode material to assemble sodium-ion half-cells and its electrochemical performance was tested.

[0063] The preparation process and electrochemical performance of the undoped porous carbon anode material electrode sheet are as follows: Appropriate amounts of negative electrode material, polyvinylidene fluoride, acetylene black, and N-methylpyrrolidone were weighed at a mass ratio of 7:2:1. After ball milling at 300 rpm for 2 h, copper foil was uniformly coated onto the mixture, and the battery electrode was obtained after vacuum drying at 80℃ for 24 h. Using the obtained battery electrode as the working electrode and a sodium sheet as the counter electrode, sodium-ion button cells were assembled in a glove box. After assembly, the cells were allowed to stand for 12 h before their electrochemical performance was measured.

[0064] The undoped porous carbon anode material prepared exhibits the following cycle performance at a current density of 0.1 A / g: Figure 4 As shown in CN, the initial discharge specific capacity is 800 mAh / g, and the discharge specific capacity after 100 cycles is 240 mAh / g.

[0065] Compared to Example 1, the discharge specific capacity of the battery in this comparative example without oxygen / sulfur doping modification is significantly reduced. This is because after oxygen / sulfur doping modification in Example 1, the carbon material has a porous framework structure and a high content of edge heteroatoms, with an oxygen content of 7.66 at% and a sulfur content of 10.61 at%. The porous, defective, and disordered microcrystalline structure on the material surface provides adsorption and sodium storage active sites for the asphalt material; simultaneously, oxygen exists in the form of carbonyl groups, while sulfur exists in the form of oxidized sulfur (C-SO₄). x -C) and thiophene-type sulfur (CSC 2p) 3 / 2 and CSC 2p 1 / 2 The presence of sodium in the form of ) with a high doping content of edge heteroatoms (10-18 at.%) improves sodium storage capacity and sodium ion kinetics.

[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-specific-capacity oxygen / sulfur co-doped porous carbon anode material, characterized in that, Includes the following steps: (1) Add asphalt and sulfur additives to the reactor and fill it with a mixture of oxygen and nitrogen gas to carry out a hot-stirred oxygen / sulfur co-doping polymerization reaction to obtain modified polymerized asphalt; (2) The modified polymeric asphalt obtained in step (1) and the micron-sized molten salt template are ball-milled and mixed evenly to obtain a solid mixture. The micron-sized molten salt template is a mixed salt of sodium chloride and potassium chloride with a mass ratio of 1:(0-1). Under a nitrogen atmosphere, the solid mixture is placed in a tube furnace for high-temperature carbonization treatment. After cooling, it is washed with deionized water, filtered, and vacuum dried to obtain a high specific capacity oxygen / sulfur co-doped porous carbon anode material.

2. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 1, characterized in that: The asphalt in step (1) is any one or more of medium-low temperature coal tar pitch, high temperature coal tar pitch, petroleum asphalt, and coal liquefaction asphalt.

3. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 2, characterized in that: The sulfur additive in step (1) is any one or more of sublimed sulfur, thiourea, and ammonium sulfate.

4. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 1, characterized in that: In step (1), the mass ratio of asphalt to sulfur additive is 1:(0.1-5); the volume ratio of oxygen to nitrogen is 1:(1-5); and the initial pressure of the oxygen and nitrogen mixture is 0.1-2 MPa.

5. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 1, characterized in that: In step (1), the polymerization reaction temperature is 150-220℃, the time is 1-5h, and the stirring rate is 100-300r / min.

6. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 1, characterized in that: In step (2), the mass ratio of modified polymeric asphalt to micron-sized molten salt template is 1:(10-20); the ball milling speed is 100-300 r / min, and the time is 2-4 h; the carbonization temperature is 600-800℃, and the time is 1-4 h.

7. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 1, characterized in that: The average particle size of the micron-sized molten salt template in step (2) is 5-8 μm.

8. The method for preparing high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 7, characterized in that: The micron-sized molten salt template is prepared by recrystallization, which includes the following steps: a prepared supersaturated mixed salt solution is gradually added dropwise to anhydrous ethanol, stirred to precipitate white crystals, and then filtered and dried to obtain the micron-sized molten salt template.

9. The high specific capacity oxygen / sulfur co-doped porous carbon anode material prepared by the method according to any one of claims 1-8, characterized in that: The high specific capacity oxygen / sulfur co-doped carbon anode material has a three-dimensional honeycomb porous framework structure composed of ultrathin carbon nanosheets; the percentage content of oxygen / sulfur heteroatoms at the edge of the carbon nanosheets is 10-20 at.%.

10. The application of the high specific capacity oxygen / sulfur co-doped porous carbon anode material according to claim 9 in sodium-ion batteries or lithium-ion batteries.

Citation Information

Patent Citations

  • Fluorination method of coal pitch-based carbon material and application of coal pitch-based carbon material in sodium ion battery

    CN115893373A

  • High-power asphalt-based sodium ion battery carbon negative electrode material as well as preparation method and application thereof

    CN117125694A