Electrolyte preparation for flow batteries
By directly using ammonium vanadate as raw material, combined with dissolution and recrystallization or adsorption treatment, the problems of energy consumption and vanadium loss in the preparation of vanadium redox flow battery electrolytes have been solved, achieving efficient and stable electrolyte preparation and simplifying the process.
Patent Information
- Application Number
- CN202410111904.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-26
AI Technical Summary
Existing methods for preparing electrolytes for vanadium redox flow batteries suffer from high energy consumption, long processing time, significant vanadium loss, and complex processes. In particular, the calcination process in the chemical method is energy and time-consuming, while the electrolysis method suffers from vanadium loss and requires sophisticated equipment.
Using ammonium vanadate as raw material, impurities are removed through dissolution, recrystallization, or adsorption treatment, avoiding the calcination process, and high-purity electrolyte is directly prepared. This includes dissolution and impurity removal steps, using a mixture of acid solvents and reducing agents, combined with low-temperature recrystallization or adsorption membrane treatment to control vanadium loss and improve purity.
It achieves energy saving, high production efficiency, high vanadium utilization, good stability of the prepared electrolyte, high total vanadium concentration, avoids crystal precipitation, simplifies the process flow, and reduces energy consumption and time consumption.
Smart Images

Figure CN117673426B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new energy, specifically relating to the preparation of electrolytes in energy storage devices, and more specifically, to the preparation of an electrolyte for a flow battery containing vanadium. Background Technology
[0002] A flow battery is a type of battery in which both the positive and negative electrode active materials are in liquid form. It differs from other electrochemical systems primarily in that the main energy source in this battery is the liquid active materials at the positive and negative electrodes, rather than solid materials in the conventional sense. The solutions of the positive and negative electrode active materials are stored in two separate containers. During operation, these solutions are circulated into the battery stack via pumps, where a battery reaction occurs, converting chemical energy into electrical energy.
[0003] Currently, vanadium redox flow batteries, especially all-vanadium redox flow batteries, have shown great promise in solar and wind energy storage, grid peak shaving, remote power supply systems, and uninterruptible power supplies due to their advantages such as pollution-free operation, long lifespan, high energy conversion efficiency, and simple maintenance. They are a crucial energy storage method for developing new energy sources. Furthermore, compared to traditional batteries, vanadium redox flow batteries, especially all-vanadium redox flow batteries, use vanadium ion reactions at both the positive and negative electrodes, eliminating cross-contamination and capacity loss.
[0004] Electrolyte, as a carrier of active materials, is one of the most important components in (all) vanadium redox flow batteries. The performance and concentration of the electrolyte directly affect the energy density of the battery. How to obtain high-performance vanadium electrolytes has become a hot research topic for researchers around the world.
[0005] The preparation methods of vanadium electrolytes generally include chemical synthesis and electrolysis. Chemical synthesis offers the advantage of simple production equipment, but the solid dissolution rate is slow, and various additives may be used during the reaction, raising concerns about the purity and performance of the vanadium electrolyte. Electrolysis can continuously produce high-concentration vanadium electrolytes in large quantities, is simple to operate, and is easy to industrialize. However, electrolysis also has disadvantages such as slow reaction rate, high equipment requirements, high energy consumption, and high cost.
[0006] In actual industrial production, vanadium oxides (such as V₂O₅) are usually used as raw materials or intermediate raw materials. For example, ammonium polyvanadate or ammonium metavanadate can be heat-treated to obtain vanadium oxides of satisfactory purity, which are then dissolved in acid to prepare electrolytes.
[0007] Reference 1 discloses an all-vanadium redox flow battery electrolyte and its preparation method, which includes preparing vanadium-containing oxide by heating ammonium metavanadate to 350-550℃; preparing an electrolyte precursor by using the vanadium-containing oxide; and electrolyzing the electrolyte precursor using an asymmetric electrolysis device to obtain a 3.5 valence electrolyte.
[0008] Reference 2 discloses a method for preparing vanadium electrolyte for all-vanadium flow batteries from vanadium-containing raw materials in a short process. The method includes extracting vanadium from vanadium-containing raw materials and removing impurities, then preparing ammonium metavanadate by passing it through ammonium salt, followed by calcination to obtain vanadium oxide, and then mixing it with sulfuric acid to obtain the electrolyte.
[0009] Reference 3 discloses a system and method for producing high-purity, high-activity vanadium electrolyte. High-purity vanadium oxychloride is converted into ammonium salt by fluidized bed gas-phase ammoniation. Subsequently, the ammonium salt is reduced to low-valence vanadium oxide with an average valence of 3.5 in another fluidized bed. Clean water and sulfuric acid are added to dissolve the oxide, and ultrasonic activation is further used to obtain a 3.5 valence vanadium electrolyte.
[0010] Reference 4 uses soluble vanadium salt as raw material, removes impurities through ion exchange resin, precipitation and other methods, and then obtains vanadium oxysulfate electrolyte by calcining and reducing the precipitate.
[0011] In addition, methods for preparing electrolytes using pentavalent vanadium stock solutions have also been reported, for example: References 5 and 6 describe the preparation of vanadium oxysulfate solution from pentavalent vanadium stock solution through steps such as impurity removal, precipitation, reduction, and extraction.
[0012] Furthermore, reference 7 discloses a method for preparing an electrolyte using ammonium metavanadate as a raw material. In this method, ammonium metavanadate and diethyldithiocarbamate are mixed to form a stock solution. Then, impurities in the stock solution are precipitated and separated using a purification agent. The stock solution with separated impurities is mixed with sulfuric acid and then electrolyzed to obtain the electrolyte. In this process, ammonium metavanadate is used directly as a raw material, and no vanadium oxide is used in the process.
[0013] Although the above research has made some progress on the process of preparing electrolytes for (all) vanadium redox flow batteries, there is still room for further improvement in terms of preparation efficiency and convenience.
[0014] References: Reference 1: CN116154244A Reference 2: CN115621515A Reference 3: CN106257726A Reference 4: CN106129442A Reference 5: CN110474077A Reference 6: CN104362360A Reference 7: CN114438514A. Summary of the Invention
[0015] The problem the invention aims to solve Through continuous practice with existing technologies, the inventors of this invention have discovered that, for the preparation of electrolytes for vanadium-containing flow batteries, especially in chemical methods, as mentioned in references 1 to 4 above, although different paths can be tried to meet different needs, the process still involves calcining vanadium oxides (such as V2O5) and then mixing them with acid to obtain the electrolyte, which presents problems in terms of energy consumption and processing time.
[0016] Furthermore, references 5 and 6 require the use of specific raw materials as the stock solution for subsequent processing, which poses certain constraints for industrial production conditions. Moreover, the entire process is not exactly simple, and in particular, there is a significant problem of vanadium loss during the processing.
[0017] Furthermore, regarding reference 7, although ammonium metavanadate can be conveniently used as a raw material and the intermediate process does not require the preparation of vanadium oxide, the process of removing impurities by precipitation also presents the problem of vanadium loss.
[0018] In addition, methods such as evaporation crystallization, alkaline precipitation, or extraction have been reported for the purification of substances such as vanadium oxysulfate, but these methods cannot be considered economical in terms of energy saving and environmental protection.
[0019] Therefore, based on the problems existing in the preparation of electrolytes in the field, the present invention provides a method for preparing flow battery electrolytes via ammonium vanadate. This method not only has a simple process flow, but also avoids the energy and time consumption of processes such as calcination, and can maximize the utilization rate of vanadium, thereby obtaining a high-quality vanadium-containing flow battery electrolyte.
[0020] Solution for solving the problem Through long-term practical research, the inventors discovered that the above-mentioned technical problems can be solved by implementing the following technical solution: [1]. This invention first provides a method for preparing a vanadium-containing electrolyte, wherein the method includes the following steps: The dissolution process and the impurity removal process; In the dissolution step, the vanadium-containing raw material is directly mixed with a solvent and a reducing agent to obtain a mixed system. The vanadium-containing raw material includes one or more ammonium vanadate compounds, and the solvent includes acidic solvents. In the impurity removal step, at least ammonium-containing impurities are removed from the mixed system by recrystallization of the impurity compound, or at least ammonium-containing impurities are removed from the mixed system by adsorption treatment to obtain a purified electrolyte system.
[0021] [2]. According to the method of [1], wherein the dissolution step includes dissolving the vanadium-containing raw material in the mixture under heating conditions.
[0022] [3]. The method according to [1] or [2], wherein the solvent is one of sulfuric acid, hydrochloric acid or a mixture thereof.
[0023] [4]. The method according to any one of [1] to [3], wherein, in the dissolution step, the amount of the reducing agent is sufficient to reduce all pentavalent vanadium ions in the mixed system.
[0024] [5]. The method according to any one of [1] to [4], wherein the mass ratio of the vanadium-containing raw material to the solvent in the dissolution step is 1:0.5 to 1:5.
[0025] [6]. The method according to any one of [1] to [5], wherein, in the step of removing impurities, the recrystallization temperature is -25°C to 5°C.
[0026] [7]. In the method according to [6], the recrystallization is carried out by gradient cooling; the pH of the mixed system during recrystallization is below 6.
[0027] [8]. The method according to any one of [1] to [7], wherein the adsorption treatment in the impurity removal step uses a porous membrane.
[0028] [9]. The method according to any one of [1] to [8], wherein the method further comprises an electrolysis step after the impurity removal step, the electrolysis step comprising one or two of the following steps: i. Perform electrolysis to control the average valence of vanadium ions in the purified electrolyte system; ii. Perform electrolysis to further remove other metal ions from the purified electrolyte system. Optionally, step i is performed in the presence of an activator.
[0029]
[10] . Furthermore, the present invention also provides a method for preparing an electrolyte for a vanadium redox flow battery, wherein the method comprises the method described in any one of [1] to [9] above.
[0030] The effects of the invention
[0031] By implementing the above technical solution, the present invention can achieve the following technical effects: ① The present invention uses non-oxide vanadium-containing raw materials (such as ammonium metavanadate, ammonium polyvanadate, etc.) as initial raw materials. In the whole process, there is no need to calcine the above-mentioned vanadium-containing raw materials to prepare vanadium oxides. Therefore, it has more economic advantages in terms of energy saving and production efficiency.
[0032] ② In the impurity removal step of this invention, the method of adding impurity removal agents to cause impurities to precipitate or solvent extraction of vanadium-containing compounds is avoided. Instead, the impurity components are removed by recrystallization or adsorption separation, which not only reduces the loss of vanadium, but also improves the purity of the processed material and improves the processing efficiency. ③ The vanadium-containing electrolyte prepared by this method can improve the reaction rate, with a total vanadium concentration of 1-5 mol / L. Moreover, the electrolyte has good stability and electrochemical activity, and no crystal precipitation occurs at low temperatures (<10℃). Attached Figure Description
[0033] Figure 1 : A process flow diagram of one embodiment of the present invention. Detailed Implementation
[0034] The present invention will now be described in detail. The descriptions of the technical features described below are based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that: In this specification, the range of values referred to as "value A to value B" refers to the range including the endpoint values A and B.
[0035] In this specification, the numerical range indicated by "above" or "below" refers to the numerical range that includes the stated number.
[0036] In this specification, the word "may" has two meanings: to perform a certain process and not to perform a certain process.
[0037] In this specification, the terms "optional" or "optional" are used to indicate the use or omission of certain substances, components, procedures, application conditions, etc.
[0038] In this specification, "room temperature" or "room temperature" refers to an indoor ambient temperature of "23±2℃", and unless otherwise specified, the "viscosity" of this invention refers to the viscosity at this temperature.
[0039] All unit names used in this manual are international standard unit names, and unless otherwise stated, the "%" indicates weight or mass percentage.
[0040] In this specification, the term "substantially" is used to indicate that the standard deviation from the theoretical model or theoretical data is within a range of 5%, preferably 3%, and more preferably 1%.
[0041] In this specification, the terms “comprising” and / or “including” are used to indicate the presence of features, steps, operations, devices, components and / or combinations thereof.
[0042] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "implementation," etc., refer to specific elements (e.g., features, structures, properties, and / or characteristics) related to that embodiment, which are included in at least one of the embodiments described herein and may or may not be present in other embodiments. Furthermore, it should be understood that these elements may be combined in any suitable manner in various embodiments.
[0043] This invention provides a convenient, efficient, economical and environmentally friendly method for preparing vanadium-containing electrolytes, which is particularly suitable as a method for preparing electrolytes for all-vanadium redox flow batteries.
[0044] This invention is mainly based on the following insights: Although vanadium-containing raw materials such as ammonium metavanadate have been used in the preparation of electrolytes for flow batteries, these metal salt compounds are typically converted into vanadium oxides through calcination, followed by acid dissolution. However, this process is uneconomical in terms of energy consumption and production time. Furthermore, while attempts have been made to use vanadium-containing raw materials such as ammonium metavanadate directly, these processes require rapid precipitation with impurity-removing agents or organic solvent extraction with the addition of alkali. Such processes introduce additional impurities and cause significant vanadium loss. More importantly, these methods are detrimental to the process, especially to the stability of the product's properties.
[0045] Therefore, a simpler and more economical synthetic route should be designed. It has been found that by starting with vanadium-containing raw materials that are not vanadium oxides, and then dissolving them followed by (low-temperature) recrystallization or adsorption separation, purified vanadium-containing electrolytes can be obtained relatively efficiently without the introduction of additional additives. In this process, there is no significant loss of vanadium, and the purity of the obtained vanadium electrolyte meets the requirements. It exhibits good stability and electrochemical activity, and no crystal precipitation occurs even at lower temperatures (e.g., below 10°C).
[0046] -First aspect- In a first aspect, the present invention provides a method for preparing a vanadium-containing electrolyte for a flow battery, the method mainly including a dissolution step and an impurity removal step.
[0047] (The dissolving step) The dissolution step of this invention mainly involves dissolving the vanadium-containing raw material using an acidic solvent.
[0048] Vanadium-containing raw materials The vanadium-containing raw materials used in this invention mainly refer to soluble salts of vanadium that are not vanadium oxides. Here, soluble salts primarily refer to salts with a solubility of 10g or more in 100ml of aqueous solution under acidic conditions at room temperature.
[0049] For such salts, the present invention may use one or more ammonium vanadate compounds, preferably, the vanadium-containing raw materials of the present invention include one or more of ammonium metavanadate, ammonium polyvanadate, etc.
[0050] In principle, there are no particular restrictions on the purity of the vanadium-containing raw materials mentioned above. In some preferred embodiments, the purity of the vanadium-containing raw materials is 95% by mass or more, more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0051] Furthermore, there are no particular limitations on the source of the aforementioned vanadium-containing raw materials such as ammonium metavanadate and ammonium polyvanadate. For example, they can be obtained by reacting vanadate with ammonium salt and then precipitating them.
[0052] acid solvents For the acid solvents that can be used in this invention, acid solvents commonly used in the preparation of flow battery electrolytes can generally be selected, typically selected from sulfuric acid, hydrochloric acid or mixtures thereof.
[0053] Examples of sulfuric acid include dilute sulfuric acid with a mass concentration of 70% or less. Preferably, the concentration of the sulfuric acid is 30-70% by mass, and more preferably 40-65% by mass.
[0054] Examples of hydrochloric acid include hydrochloric acid solutions with a mass concentration of less than 30% by mass. Preferably, the concentration of the hydrochloric acid can be 10 to 25% by mass, and more preferably 15 to 20% by mass.
[0055] Dissolve In the dissolution step of the present invention, the above-mentioned vanadium-containing raw material is mixed with an acid solvent to obtain a mixed system to dissolve the vanadium-containing raw material.
[0056] In some specific embodiments of the present invention, the dissolution is carried out under one or more conditions of heating, hot pressing, and stirring. From the perspective of rapid and complete dissolution, the above-mentioned dissolution can be carried out under heating conditions, and the heating temperature can be controlled at 50-80°C. Furthermore, in the case of a high-pressure reactor, even higher heating temperatures are permissible.
[0057] Furthermore, regarding the usage ratio of the aforementioned vanadium-containing raw materials and solvents, in some specific implementation schemes, the mass ratio of the two can be 1:0.5 to 1:5, preferably 1:0.8 to 1:1.2, and more preferably 1:0.9 to 1:1.1.
[0058] Furthermore, from the perspective of preparing vanadium with a suitable valence and increasing the solubility of vanadium-containing compounds, the dissolution step is carried out in the presence of a reducing agent.
[0059] The reducing agent that can be used in the above-described mixed system according to the present invention may include solids, gases, etc., that have reducing properties. Preferably, one or more of organic compounds and inorganic compounds with reducing properties can be used. In some specific embodiments of the present invention, the reducing agents that can be listed include one or more of oxalic acid, citric acid, sulfites, diethyldithiocarbamate, hydrogen, ammonia, methane, hydrogen sulfide, and sulfur dioxide. Preferably, the reducing agent is selected from one or more of oxalic acid, sulfites, and diethyldithiocarbamate.
[0060] There are no particular restrictions on the amount of reducing agent used. The total amount of reducing agent used should be such that all the pentavalent vanadium in the above mixed system is reduced. The result of the reduction can be tetravalent vanadium or a mixture of tetravalent and trivalent vanadium.
[0061] In some specific implementations, a solution system containing vanadium compounds is obtained through a dissolution step.
[0062] Such vanadium-containing compounds mainly include one or more of VOSO4 and VOCl2 as tetravalent vanadium, as well as V2(SO4)3 and VCl3, which may also include trivalent vanadium.
[0063] In some preferred embodiments, based on the total amount of vanadium atoms in the aforementioned vanadium-containing compound, the content of tetravalent vanadium finally obtained in the solvent step is 1.8 mol / L or more, preferably 2.0 mol / L or more, or 2.2 mol / L or more.
[0064] (Steps for impurity removal) In the impurity removal step of the present invention, the main focus is on removing the impurity compounds generated in the dissolution step. These impurity compounds are mainly ammonium salts, such as ammonium sulfate and ammonium chloride.
[0065] For methods of removing these impurities, the present invention includes separation methods such as recrystallization or adsorption treatment.
[0066] recrystallization method The main method for recrystallization is to remove impurity compounds in the mixture obtained from the above dissolution step by crystallizing them under low temperature conditions, thereby removing them through solid-liquid separation.
[0067] Furthermore, in some preferred embodiments of the present invention, from the perspective of improving recrystallization efficiency, the solid content of the above-mentioned mixed system can be adjusted before cooling recrystallization. This can be achieved by removing some water through heating, reduced pressure evaporation, etc., so that the mixed system has a suitable solid content. In some specific embodiments, before recrystallization, the solid content of the mixed system can be 50% by mass or more, preferably 55% by mass or more, and more preferably 60-80% by mass.
[0068] In addition, from the perspective of fully separating impurities during recrystallization, the pH value of the mixed system can be adjusted to below 6, preferably below 5, for example, pH=1 to 4.
[0069] The operating temperature for recrystallization can be -25℃ to 5℃, preferably -25℃ to 0℃, such as -20℃, -15℃, -10℃, etc. Too high a temperature will result in poor recrystallization or excessively long operation time, while too low a temperature will increase the difficulty of temperature control.
[0070] In some specific embodiments of the present invention, the recrystallization can be carried out by cooling down from the temperature of the above-mentioned dissolution step until the recrystallization temperature is reached.
[0071] There are no particular restrictions on the cooling method in principle, but from the perspective of maximizing the recrystallization of impurities, the cooling rate can be controlled at 1 to 5 °C / min, preferably 2 to 4 °C / min. Furthermore, in some more preferred embodiments, recrystallization can be fully achieved through gradient cooling.
[0072] In addition, in some other specific implementations, from the perspective of sufficient crystallization, seed crystals for inducing crystallization can also be added to the mixed system undergoing recrystallization.
[0073] Furthermore, there is no particular limitation on the recrystallization time (starting from the cooling start point). It can be determined based on the temperature change rate and crystal precipitation. In some preferred embodiments, when the temperature is cooled to the endpoint temperature, it can usually be held for 0.5 to 3 hours.
[0074] For the solid-liquid separation after recrystallization, the vanadium can be removed by filtration to obtain a solution system containing the aforementioned vanadium compound.
[0075] Adsorption method In the adsorption treatment step of the present invention, impurities (ammonium salts) can be separated by purification or adsorption through adsorbent or adsorption membrane.
[0076] The adsorbents or membranes used in this invention may include inorganic adsorbents (membranes), organic adsorbents (membranes), or inorganic / organic composite adsorbents (membranes). In some preferred embodiments of this invention, adsorption membranes can be used for the adsorption and separation of impurities.
[0077] There are no particular restrictions on the shape of the membrane in principle; for example, it can be a sheet membrane or a tubular membrane.
[0078] From the perspective of adsorption selectivity, the porous membrane that can be used in this invention can be an organic membrane with anionic groups, such as organic resin membranes with sulfonated groups or phosphoric acid groups.
[0079] In addition, during the adsorption step, the temperature of the mixed system to be treated can be 15 to 40°C, preferably 20 to 30°C; and the pH value of the mixed system to be treated can be below 6, preferably 5.5 to 4.5.
[0080] After the impurity removal steps of the present invention described above, a purified electrolyte system is obtained. In some specific embodiments, the concentration of ammonium salt in the electrolyte system is typically controlled to be below 20 mg / L, preferably below 15 mg / L, and more preferably below 10 mg / L. In other specific embodiments, the ammonium salt content, based on the total mass of all dry matter in the system, is below 0.02% by mass, preferably below 0.01% by mass.
[0081] (The steps of electrolysis) In some preferred embodiments of the present invention, the purified electrolyte system obtained in the above steps can be further subjected to electrolysis.
[0082] The electrolysis steps that can be used in this invention include one or two of the following steps: i. Perform electrolysis to control the average valence of vanadium ions in the purified electrolyte system; ii. Perform electrolysis to further remove other metal ions from the purified electrolyte system.
[0083] Step i There are no particular limitations on the specific implementation of step i, and it can be carried out in a conventional electrolytic cell in the art.
[0084] In some specific implementations, the electrolyte to be treated can be placed in the negative electrode of the electrolytic cell, and an acid solution, such as hydrochloric acid or sulfuric acid, can be placed in the positive electrode. Electrolysis is then performed at a specific current density, optionally 5–40 mA / cm². 2 .
[0085] There is no particular limitation on the endpoint of electrolysis in principle; it depends on the final average valence of vanadium ions in the electrolyte. In some preferred embodiments, the average valence of vanadium ions in the electrode solution at the negative electrode can be controlled to 3.5 ± 0.1, preferably 3.5 ± 0.05, through electrolysis.
[0086] Step ii Step ii can be performed before or after step i. Step ii removes impurity metal ions other than vanadium from the electrolyte. In some specific embodiments, these other metal ions may be selected from one or more of Au ions, Ag ions, Pt ions, Cu ions, Zn ions, Sn ions, Ni ions, etc.
[0087] For the specific implementation methods that can be adopted in step ii above, the present invention fully cites the purification method disclosed in patent document CN110858655 A.
[0088] (Other ingredients) The above method yields a finished electrolyte, which can be used directly or with further modifications in flow batteries as needed. In some specific embodiments, the finished electrolyte includes one or a mixture of two of VOSO4 and V2(SO4)3, and may also include one or a mixture of two of VOCl2 and VCl3. Furthermore, the total concentration of vanadium ions in the finished electrolyte can be 1–8 mol / L, preferably 2–5 mol / L.
[0089] In some specific embodiments of the present invention, from the perspective of promoting the conversion of different valence states of vanadium ions, an activator can also be added to the electrolyte.
[0090] There are no particular restrictions on when to add the activator; it can be done before, during, or after the electrolysis step described above.
[0091] The activator can be a component of non-metallic ions or metallic ions, which can be one or more ions derived from P, N, B, Ni, Mo, Mn, and Pb. In some preferred embodiments, the content of these metallic ions in the electrolyte can be 0.1 ppm or more, or 0.3 ppm or more, or 0.5 ppm or more, or 0.7 ppm or more, or 1.0 ppm or more, or 3.0 ppm or more, or 10 ppm or more, or 30 ppm or more, or 50 ppm or more, and can be less than 800 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm.
[0092] -Second aspect- Furthermore, a second aspect of the present invention also discloses a method for preparing an electrolyte for a vanadium redox flow battery, the method comprising the steps of the above-described method for preparing a vanadium-containing electrolyte for a flow battery.
[0093] In addition, the composition or characteristics of the vanadium redox flow battery can be adjusted without restriction according to the actual needs of the battery. Such adjustments include: adjusting the electrolyte acidity, adjusting the electrolyte concentration, adding other electrolyte components, and adjusting the average valence state of vanadium ions in the electrolyte.
[0094] Example The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0095] Example 1: A method for preparing tetravalent vanadium electrolyte using ammonium metavanadate as raw material and sulfuric acid (crystallization method). Measure 280ml of deionized water, add 120ml of 98% concentrated sulfuric acid, then add 100g of ammonium metavanadate raw material and 80g of oxalic acid. Heat and stir. After the reaction is complete, cool to room temperature, filter to remove insoluble matter, and place the filtrate at -20 degrees Celsius for 48 hours for recrystallization. Filter again. The filtrate is tetravalent vanadium electrolyte.
[0096] Example 2: A method for preparing tetravalent vanadium electrolyte using ammonium metavanadate as raw material and sulfuric acid (membrane adsorption method). Measure 280 ml of deionized water, add 120 ml of 98% concentrated sulfuric acid, then add 100 g of ammonium metavanadate raw material and 80 g of oxalic acid. After the reaction is complete, cool to room temperature, filter to remove insoluble matter, and pass the filtrate through an organic composite adsorption membrane to adsorb specific NH4. + The ions were filtered out as a tetravalent vanadium electrolyte.
[0097] Example 3: A method for preparing tetravalent vanadium electrolyte using ammonium metavanadate or ammonium polyvanadate as raw materials and hydrochloric acid (crystallization method). Measure 425 ml of concentrated hydrochloric acid, add 125 g of ammonium polyvanadate raw material, and then add 75 g of oxalic acid. After the reaction is complete, cool to room temperature, filter to remove insoluble matter, and place the filtrate at -20 degrees Celsius for 48 hours to recrystallize. Filter again, and the filtrate is tetravalent vanadium electrolyte.
[0098] Comparative Example 1: Conventional method for preparing electrolyte: Using ammonium metavanadate as the same raw material as in the example, vanadium pentoxide is prepared by heating, and then mixed with acid to prepare electrolyte.
[0099] Weigh 200g of ammonium metavanadate and calcine it at high temperature to obtain vanadium pentoxide. Weigh 115g of vanadium pentoxide, add 430ml of concentrated hydrochloric acid, heat and stir, then add 60g of oxalic acid. After the reaction is complete, cool and filter. Place the filtrate at -20 degrees Celsius for 48 hours, filter, and then add an appropriate amount of concentrated sulfuric acid according to the sulfate requirement to obtain tetravalent vanadium electrolyte.
[0100] Comparative Example 2: Using ammonium metavanadate, the same as in the example, as the raw material, the electrolyte was obtained by dissolving it in sulfuric acid, precipitating impurities with a precipitant, and then filtering.
[0101] Take 425 ml of concentrated hydrochloric acid, add 150 g of ammonium metavanadate, then add 120 g of oxalic acid. After the reaction is complete, add an appropriate amount of precipitant to completely precipitate the impurities, and then filter to obtain tetravalent vanadium electrolyte.
[0102] Performance Comparison : Table 1
[0103] It should be noted that although the technical solution of the present invention has been described with specific examples, those skilled in the art will understand that the present invention should not be limited thereto.
[0104] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.
[0105] Industrial applicability The method for preparing the vanadium-containing electrolyte of the present invention can be applied industrially to prepare electrolytes for all-vanadium redox flow batteries.
Claims
1. A method for preparing a vanadium-containing electrolyte, characterized in that, The method includes the following steps: The dissolution process and the impurity removal process; In the dissolution step, the vanadium-containing raw material is mixed with a solvent and a reducing agent to obtain a mixed system. The vanadium-containing raw material includes one or more ammonium vanadate compounds, and the solvent includes acidic solvents. In the impurity removal step, at least ammonium-containing impurities are removed from the mixed system by recrystallization of the impurity compound to obtain a purified electrolyte system. In the impurity removal step, the recrystallization temperature is -25℃ to 5℃, the pH value of the mixed system during recrystallization is below 6, the cooling rate during recrystallization is 1 to 5℃ / min, and when the temperature drops to the endpoint temperature, it is held for 0.5 to 3 hours.
2. The method of claim 1, wherein, The dissolution step includes dissolving the vanadium-containing raw material in the mixed system under heating conditions.
3. The method according to claim 1 or 2, characterized in that, The solvent is one of sulfuric acid, hydrochloric acid, or a mixture thereof.
4. The method according to claim 1 or 2, characterized in that, In the dissolution step, the amount of reducing agent used is sufficient to reduce all pentavalent vanadium ions in the mixed system.
5. The method according to claim 1 or 2, characterized in that, In the dissolution step, the mass ratio of the vanadium-containing raw material to the solvent is 1:0.5 to 1:
5.
6. The method according to claim 1 or 2, characterized in that, In the impurity removal step, the recrystallization temperature is -25℃ to 0℃.
7. The method according to claim 6, characterized in that, The recrystallization is carried out via gradient cooling; the pH of the mixed system during recrystallization is 1 to 5.
8. The method according to claim 1 or 2, characterized in that, The method further includes an electrolysis step after the impurity removal step, the electrolysis step comprising one or two of the following steps: i. Perform electrolysis to control the average valence of vanadium ions in the purified electrolyte system; ii. Perform electrolysis to further remove other metal ions from the purified electrolyte system. Optionally, step i is performed in the presence of an activator.
9. A method for preparing an electrolyte for an all-vanadium redox flow battery, characterized in that, The method includes the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparing method of vanadium redox flow battery electrolyte
CN104362360A
Method for preparing all-vanadium redox flow battery electrolyte by combination of resin exchange and chemical deposition
CN106129442A
System for producing high-purity high-activity vanadium electrolyte and method thereof
CN106257726A
Preparation method of novel storage battery electrolyte
CN110474077A
Method and device for purifying electrolyte of flow battery
CN110858655A