In-situ polymerized electrolyte based on dox monomer, preparation method and application thereof
By using DOX monomers to form a high-voltage resistant polymer electrolyte, the safety hazards of liquid electrolytes in lithium-ion batteries and the interface compatibility issues of ether electrolytes are solved, achieving improved energy density and safety.
Patent Information
- Application Number
- CN202311449696.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-02
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-02
AI Technical Summary
In existing lithium-ion batteries, liquid electrolytes pose safety hazards, and in-situ polymerized ether electrolytes have insufficient high voltage resistance and interface compatibility, affecting battery safety and energy density.
1,3-Dioxane (DOX) and its derivatives are used as monomers for in-situ polymerization to form a high-voltage resistant polymer electrolyte and to construct an SEI film rich in inorganic components, thereby improving the cycle stability and interfacial contact of the battery.
It improves the battery's high-voltage resistance and safety, broadens the battery's operating voltage range, enhances the electrochemical window, reduces the battery's internal resistance, improves the flammability and explosiveness of the electrolyte, and enhances the battery's energy density and cycle stability.
Smart Images

Figure CN117673460B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery materials, specifically relating to an in-situ polymerized electrolyte based on DOX monomers, its preparation method, and its applications. Background Technology
[0002] Lithium-ion batteries are widely used in small and medium-sized batteries such as portable devices and electric vehicles due to their high energy density and long lifespan, and their application areas and scale are constantly expanding. However, currently, commercial lithium-ion battery electrolytes mainly use flammable and explosive liquid electrolytes to achieve lithium-ion transport between electrodes. Liquid electrolytes present a series of safety issues during battery operation, including gas generation, leakage, flammability, and explosion. Therefore, with the rapid development of lithium batteries and the expansion of their application scenarios, higher requirements have been placed on the safety performance of lithium-ion batteries.
[0003] Solid-state lithium metal batteries, which use chemically inert solid electrolytes instead of liquid electrolytes, are considered a promising strategy for achieving high-safety lithium batteries. However, the poor solid-solid contact and interfacial compatibility of solid electrolytes result in low ionic conductivity. To improve the interfacial contact between the electrolyte and the electrode and enhance the electrolyte's lithium-ion conduction, in-situ polymerization to prepare polyether gel / solid electrolytes is proposed as an effective strategy to address both interfacial compatibility and safety concerns.
[0004] Currently, research on in-situ polymerized polyether electrolytes mainly focuses on the preparation of polyether electrolytes using the ring-opening polymerization of 1,3-dioxolane (DOL) (such as the existing technology CN116190776A). However, due to the poor high-voltage resistance of the repeating units in the chain structure of poly(1,3-dioxolane) (P-DOL) and its severe decomposition in ternary cathode materials, the application of in-situ polymer solid electrolytes in lithium batteries is seriously hindered.
[0005] Therefore, it is urgent to find an alternative technical solution to address the problems of poor high-voltage resistance and insufficient safety of the aforementioned in-situ polymerized ether electrolytes. Summary of the Invention
[0006] This invention provides an in-situ polymerized electrolyte based on DOX monomers. Through in-situ polymerization, a polymer electrolyte with high voltage resistance and certain flame retardancy is formed, and it is compatible with high-voltage cathode materials, thereby improving the energy density and safety of lithium batteries. By using 1,3-dioxane (DOX) and its derivatives as monomers for in-situ polymerization, it is possible to improve the high voltage resistance of the electrolyte and construct an SEI film rich in inorganic components, thus enhancing the cycle stability of the battery.
[0007] One object of the present invention is to provide an in-situ polymeric electrolyte based on DOX monomer, the in-situ polymeric electrolyte comprising the following raw materials: polymeric monomer, initiator and lithium salt;
[0008] The polymeric monomer is represented by the following general structural formula:
[0009]
[0010] in,
[0011] R1-R4 are independently selected from one or more of hydrogen atoms, halogens, cyano groups, nitro groups, sulfonic acid groups, C1-C8 alkyl chains, C1-C8 alkoxy chains, C1-C8 alkyl chain derivatives, or C1-C8 alkoxy chain derivatives.
[0012] In the C1-C8 alkyl chain derivatives and C1-C8 alkoxy chain derivatives, one or more hydrogen atoms on the alkyl chain or alkoxy chain are replaced by halogens.
[0013] Furthermore, the halogen is selected from one or more of F, Cl, Br, or I.
[0014] Furthermore, the polymeric monomer is selected from one or more of the following structures:
[0015]
[0016]
[0017] R5 is selected from C1-C8 alkyl chains and C1-C8 alkoxy chains.
[0018] Furthermore, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium dioxaborate, lithium difluorooxaborate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide.
[0019] Furthermore, the initiator is selected from one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, tin tetrafluoride, stannous fluoride, zinc fluoride, lithium difluorooxalate borate, copper fluoride, zinc iodide, potassium hexafluorophosphate, trifluoromethanesulfonate, and trifluoromethanesulfonate.
[0020] The present invention also provides a method for preparing the DOX-based in-situ polymeric electrolyte, wherein the method for preparing the DOX-based in-situ polymeric electrolyte includes the following steps:
[0021] S1. Dissolve the lithium salt in the polymer monomer, mix, and obtain a lithium salt solution;
[0022] S2. Add the initiator to the lithium salt solution, mix, and obtain the precursor solution;
[0023] S3. The precursor solution is heated to react and obtain the polymer electrolyte.
[0024] Furthermore, the concentration of the lithium salt is 0.5-3M.
[0025] Preferably, the concentration of the lithium salt is 0.5-1.5M.
[0026] Further, in step S1, the molar ratio of the lithium salt to the polymer monomer is 1-2:8-10.
[0027] Furthermore, the concentration of the initiator is 0.1-100 mM.
[0028] Furthermore, in step S3, the heating temperature is 35-85°C.
[0029] Preferably, in step S3, the heating temperature is 55-65°C.
[0030] Specifically, the long carbon chain structure of the 1,3-dioxane molecule in the polymer monomer of the present invention can reduce the binding ability of the P-DOX polymer chain to lithium ions and promote the transport of anions, thereby realizing the construction of an anion-derived SEI film rich in inorganic components and improving the cycle stability and high voltage resistance of the battery.
[0031] The present invention also provides a lithium-ion battery, the lithium-ion battery comprising a positive electrode, a negative electrode, a separator and the in-situ polymerized electrolyte based on DOX monomer;
[0032] The cathode material is selected from at least one of lithium iron phosphate, high-nickel ternary cathode material, lithium nickel cobalt manganese oxide, and lithium titanate.
[0033] The negative electrode material is metallic lithium;
[0034] The diaphragm is selected from at least one of polyethylene film (PE), polypropylene film (PP), cellulose film, and glass cellulose film.
[0035] The present invention has the following beneficial effects:
[0036] (1) The in-situ polymerized electrolyte based on DOX monomer described in this invention has good interfacial contact and reduces the internal resistance of the battery; in addition, the designed molecular structure effectively improves the high voltage resistance of the battery, broadens the working voltage of the battery, and is conducive to improving the energy density of the battery; it also increases the decomposition temperature and improves the high safety of the battery.
[0037] (2) The present invention uses DOX monomers, which have the characteristics of good high voltage resistance, effectively improving the problems of low decomposition temperature and narrow electrochemical window of polyether electrolytes, achieving a higher electrochemical window, and increasing the decomposition temperature of electrolytes, thereby improving the energy density and safety performance of batteries. At the same time, the electrolyte is prepared by in-situ polymerization, with no small molecule residue or little small molecule solvent residue, which greatly improves the flammability and explosiveness of electrolytes and improves the cycle stability and safety of batteries. Moreover, the polymer electrolyte of the present invention realizes the in-situ conversion of the electrode / electrolyte solid-liquid interface to solid-solid interface in the battery, which is beneficial to improve interface contact and reduce battery interface impedance. Attached Figure Description
[0038] Figure 1 Test images of Li|| stainless steel (SUS) batteries for Application Example 1, Comparative Application Example 1, and Comparative Application Example 4;
[0039] Figure 2 Coulombic efficiency diagrams of Li||Li cells for Application Example 3, Comparative Application Example 3, and Comparative Application Example 6;
[0040] Figure 3 The battery cycle performance of Li||NCM111 batteries in Application Example 2, Comparative Application Example 2, and Comparative Application Example 5 at 25°C is shown in the graph.
[0041] Figure 4 The graph shows the battery cycle performance of the Li||NCM111 battery in Application Example 2 at different rates;
[0042] Figure 5 (a) is a graph showing the battery cycle performance of the Li||NCM111 battery in Application Example 2;
[0043] Figure 5 (b) is a graph showing the battery cycle performance of the Li||LCO battery in Application Example 4;
[0044] Figure 5 (c) is a graph showing the battery cycle performance of the Li||NCM811 battery in Application Example 5. Detailed Implementation
[0045] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.
[0046] Celgard 3501 was purchased from Celgard Diaphragm Company in the United States.
[0047] Example 1
[0048] An in-situ polymeric electrolyte based on DOX monomer, the in-situ polymeric electrolyte comprising the following steps:
[0049] S1-1. At room temperature, 10.0 g of 2,2-difluoro-propanediol was slowly added dropwise to 15 mL of anhydrous 2,2-dimethoxypropane. After the addition was complete, 0.01 eq of In(OTf)3 was added as a catalyst, and the mixture was heated to 50 °C and reacted for 12 h. Then the mixture was slowly returned to room temperature. After the reaction was completed, a crude product was obtained. The crude product was purified by distillation three times at room temperature to obtain the polymer monomer 2FMDX.
[0050] The yield of the polymer monomer 2FMDX was 86%;
[0051] The chemical synthesis route for the monomer 2FMDX (5,5-difluoro-2,2-dimethyl-1,3-dioxane) is shown below:
[0052]
[0053] 1H-NMR (600MHz, CDCl3, δ / ppm): 4.02~3.84 (m, 4H), 1.92 (m, 6H).
[0054] 19F-NMR (564MHz, CDCl3, δ / ppm): -110.46~-112.48 (s, 2F).
[0055] 13C-NMR (150MHz, CDCl3, δ / ppm): 110.67~115.38, 66.09~60.32, 25.79~20.66.
[0056] S1-2. In an argon-filled glove box (H2O≤0.01ppm, O2≤0.01ppm), lithium bisfluorosulfonylimide (LiFSI) is dissolved in 1 mL of the polymer monomer 2FMDX and mixed thoroughly to obtain a lithium salt solution; wherein the molar ratio of lithium bisfluorosulfonylimide to the polymer monomer is 1:8.
[0057] S2. Dissolve 20 mmol of Al(OTf)3 in the lithium salt solution and mix thoroughly to obtain a precursor solution;
[0058] S3. The precursor solution is reacted at 60°C for 36 hours to obtain a polymer electrolyte.
[0059] Example 2
[0060] An in-situ polymeric electrolyte based on DOX monomer, the in-situ polymeric electrolyte comprising the following steps:
[0061] S1-1. At room temperature, 10.0 g of 2,2-difluoro-propanediol was slowly added dropwise to 15 mL of anhydrous dimethyl formaldehyde. After the addition was complete, 0.01 eq of In(OTf)3 was added as a catalyst, and the mixture was heated to 40 °C and reacted for 10 h. Then the mixture was slowly returned to room temperature. After the reaction was completed, a crude product was obtained. The crude product was purified by distillation three times at room temperature to obtain the polymer monomer 2FDX.
[0062] The yield of the polymer monomer 2FDX was 86%;
[0063] The synthetic route for the monomer 2FDX (5,5-difluoro-1,3-dioxane) is shown below:
[0064]
[0065] 1H-NMR (600MHz, CDCl3, δ / ppm): 4.92 (m, 2H), 4.02~3.84 (m, 4H).
[0066] 19F-NMR (564MHz, CDCl3, δ / ppm): -110.46~-112.48 (s, 2F).
[0067] 13C-NMR (150MHz, CDCl3, δ / ppm): 110.67~115.38, 66.09~60.32.
[0068] S1-2. In an argon-filled glove box (H2O≤0.01ppm, O2≤0.01ppm), lithium bisfluorosulfonylimide (LiFSI) is dissolved in 1 mL of the polymeric monomer 2FDX and mixed thoroughly to obtain a lithium salt solution; wherein the molar ratio of lithium bisfluorosulfonylimide to the polymeric monomer is 1:8.
[0069] S2. Dissolve 20 mmol of Al(OTf)3 in the lithium salt solution and mix thoroughly to obtain a precursor solution;
[0070] S3. React 80 μL of the precursor solution at 60 °C for 36 h to obtain the polymer electrolyte.
[0071] Example 3
[0072] This embodiment provides an in-situ polymeric electrolyte based on DOX monomer. The only difference between this embodiment and Example 1 is that in step S1-1, 2,2-difluoro-propanediol is replaced with an equal mass of 2,2-dimethyl-propanediol to obtain 4MDX as the polymeric monomer. Other raw materials, amounts, and preparation methods are the same as in Example 1.
[0073] The synthetic route for the monomer 4MDX (5,5-dimethyl-2,2-dimethyl-1,3-dioxane) is shown below:
[0074]
[0075] Example 4
[0076] This embodiment provides an in-situ polymeric electrolyte based on DOX monomer. The only difference between this embodiment and Example 3 is that in step S1-1, 2,2-dimethyloxypropane is replaced with dimethylformaldehyde to obtain 2MDX as the polymeric monomer. Other raw materials, dosages, and preparation methods are the same as in Example 1.
[0077] The synthetic route for the monomer 2MDX (5,5-dimethyl-1,3-dioxane) is shown below:
[0078]
[0079] Example 5
[0080] This embodiment provides a polymer electrolyte, which differs from Example 3 only in that, in step S1-1, 2,2-difluoro-propanediol is replaced by 2-trifluoromethyl-propanediol in equal mass, and the polymer monomer is TFMDX. Other raw materials, amounts and preparation methods are the same as in Example 1.
[0081] The synthetic route for the monomer TFMDX (5-trifluoromethyl-1,3-dioxane) is shown below:
[0082]
[0083] Example 6
[0084] This embodiment provides a polymer electrolyte, which differs from Example 1 only in that, in steps S1-2, the polymer monomer 2FMDX is replaced with an equal mass of 1,3-dioxane (DOX), while the other raw materials, amounts, and preparation methods are the same as in Example 1.
[0085] Comparative Example 1
[0086] The difference between this comparative example and Example 1 is that step S3 is removed, and only the precursor solution is prepared. The other raw materials, proportions and preparation methods are the same as in Example 1.
[0087] Comparative Example 2
[0088] The difference between this comparative example and Example 1 is that in steps S1-2, the polymeric monomer 2FMDX is replaced by an equal volume of 1,3-dioxolane (DOL), while the other raw materials, proportions, and preparation methods are the same as in Example 1.
[0089] Application Example 1
[0090] In-situ polymerization assembly of Li|| stainless steel (SUS) batteries
[0091] The preparation method of the Li|| stainless steel (SUS) battery is as follows:
[0092] In a glove box under an argon atmosphere (H2O≤0.01ppm, O2≤0.01ppm), a 2032 stainless steel button cell was used. Li was used as the negative electrode, stainless steel as the positive electrode, and a Celgard-3501 separator was used to assemble the battery. 100 μL of the precursor solution obtained in step S2 of Example 1 was added, and the battery was assembled under a pressure of 900 MPa. After assembly, the battery was subjected to in-situ polymerization in an oven at 55 °C for 36 h to obtain a Li|| stainless steel (SUS) battery.
[0093] Application Example 2
[0094] In-situ polymerization assembly of Li||NCM111 cells
[0095] The preparation method of the Li||NCM111 battery is as follows:
[0096] LiNi ternary cathode material 0.33 Co 0.33 Mn 0.33 Preparation of O2 (NCM111) electrode: 2g of ternary cathode material was weighed, and then NCM111, acetylene black, and PVDF binder were mixed in a mass ratio of 80:12:8. This mixture was added to 2mL of N-methylpyrrolidone (NMP) solution and dispersed to prepare a slurry. The slurry was then uniformly coated onto aluminum foil using a 100μm scraper and subsequently vacuum-dried at 120℃ for 12h. The slurry was then sliced using a slicing machine to obtain a diameter of 12mm and a ternary cathode material loading of 2mg / cm². -2 The electrode discs were placed in the glove box for later use;
[0097] In a glove box under an argon atmosphere (H2O≤0.01ppm, O2≤0.01ppm), the prepared electrode discs were matched with copper foil and lithium metal, respectively. Celgard 3501 was used as a separator, and 100 μL of the precursor solution obtained in step S2 of Example 1 was added. The battery was assembled under a pressure of 900 MPa. After assembly, the battery was subjected to in-situ polymerization in an oven at 55 °C for 36 h to obtain Li||NCM111 battery.
[0098] Application Example 3
[0099] In-situ polymerization assembly of Li||Li batteries
[0100] The preparation method of Li||Li battery is as follows:
[0101] In a glove box under an argon atmosphere (H2O≤0.01ppm, O2≤0.01ppm), a 2032 stainless steel button cell was used, with Li as the symmetrical electrode and a Celgard-3501 separator to assemble the cell. 100 μL of the precursor solution obtained in step S2 of Example 1 was added, and the cell was assembled under a pressure of 900 MPa. After assembly, the cell was subjected to in-situ polymerization in an oven at 55 °C for 36 h to obtain a Li||Li cell.
[0102] Application Example 4
[0103] In-situ polymerization assembly of Li||LCO cells
[0104] The preparation method of the Li||LCO battery is as follows: In a glove box under an argon atmosphere (H2O≤0.01ppm, O2≤0.01ppm), a 2032 stainless steel button cell is used. Li is used as the negative electrode, lithium cobalt oxide is used as the positive electrode, and Celgard-3501 is used as the separator to assemble the battery. 100μL of the precursor solution obtained in step S2 of Example 1 is added, and the battery is assembled under a pressure of 900MPa. After assembly, the battery is subjected to in-situ polymerization reaction in an oven at 55℃ for 36h to obtain the Li||LCO battery.
[0105] Application Example 5
[0106] In-situ polymerization assembly of Li||NCM811 batteries
[0107] The preparation method of the Li||NCM811 battery is as follows:
[0108] In a glove box under an argon atmosphere (H2O≤0.01ppm, O2≤0.01ppm), a 2032 stainless steel button cell was used. Li was used as the negative electrode, ternary material (NCM811) was used as the positive electrode, and Celgard-3501 was used as the separator to assemble the battery. 100 μL of the precursor solution obtained in step S2 of Example 1 was added, and the battery was assembled under a pressure of 900 MPa. After assembly, the battery was subjected to in-situ polymerization in an oven at 55°C for 36 h to obtain the Li||NCM811 battery.
[0109] Comparative Application Example 1
[0110] The difference between this comparative application example and application example 1 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 1 in equal volume, and the in-situ polymerization reaction step is removed. Other raw materials, amounts and preparation methods are the same as in application example 1.
[0111] Comparative Application Example 2
[0112] The difference between this comparative application example and application example 2 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 1 in equal volume, and the in-situ polymerization reaction step is removed. Other raw materials, amounts and preparation methods are the same as in application example 1.
[0113] Comparative Application Example 3
[0114] The difference between this comparative application example and application example 3 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 1 in equal volume, and the in-situ polymerization reaction step is removed. Other raw materials, amounts and preparation methods are the same as in application example 1.
[0115] Comparative Application Example 4
[0116] The difference between this comparative application example and application example 1 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 2 in equal volume, while the other raw materials, amounts and preparation methods are the same as in application example 1.
[0117] Comparative Application Example 5
[0118] The difference between this comparative application example and application example 2 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 2 in equal volume, while the other raw materials, amounts and preparation methods are the same as in application example 1.
[0119] Comparative Application Example 6
[0120] The difference between this comparative application example and application example 3 is that the precursor solution of example 1 is replaced with the precursor solution of comparative example 2 in equal volume, while the other raw materials, amounts and preparation methods are the same as in application example 1.
[0121] Test Example 1
[0122] The Li|| stainless steel (SUS) batteries corresponding to Use Case 1 and Comparative Application Example 1 and Comparative Application Example 4, respectively, are used at 5mV s -1 The scanning rate was tested using the linear scanning voltammetry method on a Chenhua instrument.
[0123] Test method:
[0124] The open-circuit voltage of the Li|| stainless steel (SUS) batteries in Test Application Example 1 and Comparative Application Examples 1 and 4 was measured, with the open-circuit voltage used as the starting voltage and 6.5V as the ending voltage. The scan rate was 5mV / s. -1 After setting it up, perform a test. The test results are as follows: Figure 1 As shown;
[0125] Figure 1 Test images of Li|| stainless steel (SUS) batteries for Application Example 1, Comparative Application Example 1, and Comparative Application Example 4;
[0126] Depend on Figure 1 It can be seen that in the potential range of 2.5-4.5V, there is no obvious oxidation current in Application Example 1, indicating that in this potential range, the polymer electrolyte in the Li|| stainless steel (SUS) battery of Application Example 1 does not undergo obvious electrochemical reaction and can exist stably.
[0127] Test Example 2
[0128] Performance tests were conducted on the Li||NCM111 battery corresponding to use case 2 and comparative application examples 2 and 5, and the Li||Li battery corresponding to use case 3 and comparative application examples 3 and 6, respectively.
[0129] The results of the discharge specific capacity retention rate test of the Li||NCM111 battery corresponding to use case 2 and comparative application examples 2 and 5 are shown in Table 1.
[0130] The electrochemical performance of Li||NCM111 batteries corresponding to Application Example 2 and Comparative Application Example 2, Comparative Application Example 5, and Li||Li batteries corresponding to Application Example 3 and Comparative Application Example 3, Comparative Application Example 6 was tested at room temperature, and the results are as follows: Figure 2 and Figure 3 As shown.
[0131] Figure 2 Coulombic efficiency diagrams of Li||Li cells for Application Example 3, Comparative Application Example 3, and Comparative Application Example 6;
[0132] Figure 3 The battery cycle performance of Li||NCM111 batteries in Application Example 2, Comparative Application Example 2, and Comparative Application Example 5 at 25°C is shown in the graph.
[0133] Table 1 shows the test results of the discharge specific capacity retention rate of Li||NCM111 batteries in Application Example 2 and Comparative Application Example 2 and Comparative Application Example 5:
[0134]
[0135] As can be seen from Table 1, compared with Comparative Application Examples 2 and 5, the battery in Application Example 2 has a higher discharge specific capacity and capacity retention rate. Figure 2-3 It can be seen that Application Example 2 exhibits excellent cycle stability, which is better than that of Comparative Application Examples 2 and 5.
[0136] Test Example 3
[0137] The battery cycle performance of the Li||NCM111 battery at different rate corresponding to test case 2 is shown in the following test results. Figure 4 As shown.
[0138] Figure 4The graph shows the battery cycle performance of the Li||NCM111 battery in Application Example 2 at different rates;
[0139] from Figure 4 It can be seen that the Li||NCM111 battery using Application Example 2 exhibits excellent rate performance.
[0140] Test Example 4
[0141] The Li||NCM111 battery from Application Example 2, the Li||LCO battery from Application Example 4, and the Li||NCM811 battery from Application Example 5 were subjected to battery cycle performance tests, and the test results are as follows: Figure 5 As shown.
[0142] Figure 5 (a) is a graph showing the battery cycle performance of the Li||NCM111 battery in Application Example 2; Figure 5 (b) is a graph showing the battery cycle performance of the Li||LCO battery in Application Example 4; Figure 5 (c) is a graph showing the battery cycle performance of the Li||NCM811 battery in Application Example 5;
[0143] from Figure 5 It can be seen that the in-situ polymerized electrolyte of the batteries in Application Examples 2 and 4-5 exhibits excellent high-voltage resistance and can achieve good electrochemical performance in different cathode materials. This indicates that the in-situ polymerized electrolyte based on the present invention has good versatility and can be applied to a variety of lithium batteries.
[0144] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
[0145] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. An in-situ polymeric electrolyte based on DOX monomer, characterized in that, The in-situ polymeric electrolyte comprises the following raw materials: polymeric monomers, initiators, and lithium salts; The polymeric monomer is selected from one or more of the following structures: R5 is selected from C1-C8 alkyl chains and C1-C8 alkoxy chains.
2. The in-situ polymeric electrolyte based on DOX monomer according to claim 1, characterized in that, The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium dioxaborate, lithium difluorooxaborate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl)imide, or lithium bis(fluorosulfonyl)imide.
3. The in-situ polymeric electrolyte based on DOX monomer according to claim 1, characterized in that, The initiator is selected from one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, tin tetrafluoride, stannous fluoride, zinc fluoride, lithium difluorooxalate borate, copper fluoride, zinc iodide, potassium hexafluorophosphate, trifluoromethanesulfonate, and trifluoromethanesulfonate.
4. The method for preparing the in-situ polymeric electrolyte based on DOX monomer according to any one of claims 1-3, characterized in that, The preparation method of the DOX monomer-based in-situ polymerized electrolyte includes the following steps: S1. Dissolve the lithium salt in the polymer monomer, mix, and obtain a lithium salt solution; S2. Add the initiator to the lithium salt solution, mix, and obtain the precursor solution; S3. The precursor solution is heated to react and a polymer electrolyte is obtained.
5. The method for preparing the in-situ polymeric electrolyte based on DOX monomer according to claim 4, characterized in that, In step S1, the molar ratio of the lithium salt to the polymer monomer is 1-2:8-10.
6. The method for preparing the in-situ polymeric electrolyte based on DOX monomer according to claim 4, characterized in that, The concentration of the initiator is 0.1-100M.
7. The method for preparing the in-situ polymeric electrolyte based on DOX monomer according to claim 4, characterized in that, In step S3, the heating temperature is 35-85℃.
8. A lithium-ion battery, characterized in that, The lithium-ion battery includes a positive electrode, a negative electrode, a separator, and an in-situ polymerized electrolyte based on DOX monomers as described in any one of claims 1-3; The cathode material is selected from at least one of lithium iron phosphate, high-nickel ternary cathode material, lithium nickel cobalt manganese oxide, and lithium titanate. The negative electrode material is metallic lithium; The diaphragm is selected from at least one of polyethylene membrane, polypropylene membrane, cellulose membrane, and glass cellulose membrane.
Citation Information
Patent Citations
Gel electrolyte containing LiPF6 and DOL as well as preparation method and application of gel electrolyte
CN116190776A
All-solid-state sodium-ion battery electrolyte and preparation method thereof
CN110229365A
Compound for polymer electrolyte, polymer electrolyte, film electrode assembly, solid polymer type fuel cell and manufacturing method for polymer electrolyte