Carbon dioxide reduction composite photocatalytic material, preparation method and application
By loading copper oxide or iron oxide nanoparticles onto carbon nitride to form closely contacted heterojunctions, the problems of high synthesis complexity and cost in the existing carbon dioxide reduction reaction are solved, the catalytic activity and stability are improved, and efficient carbon dioxide reduction is achieved.
Patent Information
- Application Number
- CN202211043472.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Existing photocatalytic materials for carbon dioxide reduction reactions suffer from problems such as complex synthesis, high cost, and difficulty in large-scale application. Furthermore, severe carrier recombination leads to insufficient catalytic activity.
Using carbon nitride as the substrate semiconductor material, copper oxide or iron oxide nanoparticles are loaded and formed into a tightly contacted heterojunction through hydrothermal growth. Combined with temperature-programmed technology, carbon nitride is exfoliated in situ to promote charge separation and catalytic activity.
It improves the activity and stability of the catalyst in the CO and CH₄ generation rate during the carbon dioxide reduction process, enhances the light absorption performance and charge separation efficiency, and realizes a highly efficient carbon dioxide reduction reaction.
Smart Images

Figure CN117680176B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalysis technology, specifically relating to a carbon dioxide reduction composite photocatalytic material, its preparation method, and its application. Background Technology
[0002] With the increasing depletion of traditional fossil fuels and the escalating global climate crisis, exploring stable methods to control the total amount of carbon dioxide in the atmosphere and actively addressing the energy crisis are major issues of national and societal concern. Utilizing photocatalytic materials under mild reaction conditions of ambient temperature and pressure, driven by sunlight, to achieve the catalytic conversion of carbon dioxide into high-value-added chemicals is of crucial significance. Achieving sustainable carbon recycling using hydrocarbon fuels as energy carriers is the most ideal solution for CO2 conversion and utilization. Developing novel and efficient photocatalytic materials to construct highly efficient photocatalytic reaction systems is one of the key strategies for realizing this approach.
[0003] A prior art technology discloses a phosphorus-doped graphene quantum dot-carbon nitride pn junction photocatalyst, its preparation method, and its applications. The preparation method includes: dissolving 1,3,6-trinitrobenzene and Na2HPO4·12H2O in water to obtain a mixed aqueous solution; preparing phosphorus-doped graphene quantum dots under alkaline conditions and hydrothermal reaction; and utilizing the π-π hydrogen bonding between the phosphorus-doped graphene quantum dots and carbon nitride to form a stable composite material. The phosphorus-doped graphene quantum dots are p-type semiconductor materials, and the pn junction composite material formed with n-type carbon nitride exhibits significantly improved photogenerated charge separation rate and visible light photocatalytic activity, which can be used for visible light desorption of dyes or organic pollutants, and photocatalytic water splitting to produce hydrogen. However, this disclosed method has drawbacks: the synthesis method is relatively complex, a highly toxic PH3 gas is generated during the process, and it cannot be applied to carbon dioxide reduction reactions.
[0004] CN107308978B discloses a heterojunction interface-doped composite photocatalyst and its preparation method, wherein the prepared heterojunction interface-doped Bi 12 O 17 The Cl2 / g-C3N4 composite photocatalyst possesses the ability to convert carbon dioxide into methane under visible light. It employs g-C3N4 and Bi... 12 O 17 Cl2 nanosheet composites are more likely to form large-area heterojunctions, thereby promoting carrier separation. However, this method has the drawback of high cost of Bi-based raw materials, which hinders large-scale applications.
[0005] CN110013869A relates to a composite material of carbon nitride nanosheets supported on titanium carbide quantum dots, its preparation method, and its application. Titanium carbide quantum dots (Ti₂C₃) are uniformly distributed on the surface of carbon nitride nanosheets. The method includes: 1) synthesis of titanium carbide quantum dots; 2) adding a carbon nitride precursor to an aqueous solution of titanium carbide quantum dots obtained in step 1), stirring and mixing thoroughly, then rapidly freezing, followed by vacuum drying and calcination under an inert atmosphere to obtain a composite photocatalytic material of carbon nitride nanosheets supported on titanium carbide quantum dots. However, this disclosure has shortcomings such as complex synthesis methods and stringent conditions, and it does not demonstrate its application in carbon dioxide reduction. Summary of the Invention
[0006] To overcome the shortcomings of the prior art, the present invention provides a low-cost carbon nitride-containing catalyst for photocatalytic conversion of carbon dioxide, comprising metal oxide nanoparticles supported on carbon nitride.
[0007] Carbon nitride has a two-dimensional nanosheet structure; the metal oxide nanoparticles are copper oxide nanoparticles and / or iron oxide nanoparticles. The bonding between the metal oxide nanoparticles and carbon nitride is characterized by tight interfacial contact.
[0008] The carbon nitride in the catalyst has a two-dimensional layered structure, which helps to improve the catalyst's activity in terms of CO and CH4 generation rates and catalyst stability.
[0009] According to one embodiment of the present invention, the content of the metal oxide is 5wt%-30wt%, and the content of carbon nitride is 70wt%-95wt%, wherein copper oxide is calculated as CuO, iron oxide is calculated as Fe2O3, and carbon nitride is calculated as C3N4.
[0010] According to one embodiment of the present invention, the specific surface area of the carbon nitride is 4 m². 2 / g-10m 2 / g.
[0011] According to one embodiment of the present invention, the light absorption range of the photocatalytic material is 200nm-600nm, indicating that the material has a good response to sunlight.
[0012] Another object of the present invention is to provide a method for preparing the above-mentioned catalyst, comprising the following steps:
[0013] S1, preparation of carbon nitride;
[0014] S2. Disperse the carbon nitride prepared in step S1 in water to obtain dispersion A;
[0015] S3. Add soluble metal salt and alkaline solution to dispersion A, mix thoroughly, and then carry out hydrothermal reaction;
[0016] S4. Separate, wash and dry the product obtained in step S3 to obtain a solid product;
[0017] S5. After calcining the solid product obtained in step S4, cool it to room temperature to obtain the photocatalytic material.
[0018] According to one embodiment of the present invention, in step S1, the preparation step of the carbon nitride includes: calcining a carbon-nitrogen-containing organic compound; the calcination process is a programmed temperature increase from room temperature to the maximum calcination temperature;
[0019] In-situ exfoliation of carbon nitride was performed by programmed temperature calcination. The resulting in-situ exfoliated carbon nitride has a two-dimensional layered structure, which helps to improve the activity of the catalyst in terms of CO and CH4 generation rates and catalyst stability.
[0020] Preferably, the maximum calcination temperature is 520℃-600℃, and the heating rate is 2-10℃ / min.
[0021] Preferably, a segmented programmed heating and calcination process is adopted. The first segment of the programmed heating and calcination process is from room temperature to the first calcination temperature, with a heating rate of 2-10℃ / min. The second segment of the programmed heating and calcination process is from the first calcination temperature to the highest calcination temperature, with a heating rate of 2-10℃ / min. The first calcination temperature is 500-550℃.
[0022] Using segmented programmed heating and calcination can make the catalyst structure more uniform.
[0023] According to one embodiment of the present invention, the carbon-nitrogen-containing organic compound is one or more of melamine, dicyandiamide, and urea.
[0024] According to one embodiment of the present invention, in step S2, the dispersion method is ultrasonic dispersion.
[0025] In step S2, the weight ratio of water to carbon nitride is 5-0.5:1.
[0026] According to one embodiment of the present invention, in step S3, the metal salt is a copper salt or an iron salt; preferably, the metal salt is one or more of the chloride salt, nitrate salt, sulfate salt and soluble organic salt of the corresponding metal.
[0027] Preferably, the soluble organic salt is acetylacetone salt.
[0028] In step S3, the alkaline solution used is at least one of ammonia water, urea solution, sodium hydroxide solution, and potassium hydroxide solution; the concentration of the alkaline solution is preferably 5wt%-50wt%.
[0029] In step S3, the hydrothermal reaction temperature is 120℃-150℃, and the time is 12-48 hours. Too low a temperature and reaction time are not conducive to the crystallization of metal oxides, while too high a temperature will cause agglomeration.
[0030] Preferably, the equipment for the hydrothermal reaction is a hydrothermal reactor lined with polytetrafluoroethylene.
[0031] Through hydrothermal reaction, a tight interfacial contact is formed between copper oxide or iron oxide and carbon nitride, thereby improving charge lifetime, promoting the photocatalytic CO2 reduction process, and enhancing the CO generation rate activity and catalyst stability.
[0032] According to one embodiment of the present invention, in step S4, the washing step is to wash with water and / or ethanol respectively to remove residual anions; the drying method is to dry.
[0033] According to one embodiment of the present invention, in step S5, the calcination temperature is 200℃-300℃ and the time is 1-2 hours.
[0034] Beneficial effects:
[0035] Compared with the prior art, the advantages of the present invention are as follows:
[0036] 1. Using carbon nitride as the substrate semiconductor photocatalytic material, and directly growing copper oxide and / or iron oxide in situ hydrothermally on carbon nitride, close contact between the two semiconductors can be achieved, thereby improving charge lifetime, promoting the photocatalytic CO2 reduction process, and improving CO generation rate activity and catalyst stability.
[0037] 2. By using programmed temperature rise technology to exfoliate polymer carbon nitride in situ during the synthesis process, the growth of copper oxide or iron oxide is promoted, which is beneficial to improving the activity of CO generation rate and catalyst stability during photocatalytic CO2 reduction.
[0038] 3. Because the constructed binary composite photocatalytic material forms a heterojunction, it can overcome the problem of severe carrier recombination in single semiconductors such as carbon nitride, copper oxide, or iron oxide. At the same time, the enhanced light absorption performance, improved charge separation efficiency, and increased active sites caused by the formation of composite materials can significantly improve the photocatalytic activity of carbon dioxide reduction to CO and CH4.
[0039] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. Attached Figure Description
[0040] Figure 1 This is the X-ray diffraction (XRD) pattern of the carbon nitride / copper oxide composite material prepared in Example 1.
[0041] Figure 2This is the UV-Vis DRS of the carbon nitride / copper oxide composite material prepared in Example 1.
[0042] Figure 3 The images show the fluorescence spectra (PL) of carbon nitride prepared in Example 1 before and after being combined with copper oxide, where a and b are the fluorescence spectra of pure carbon nitride and the composite material, respectively.
[0043] Figure 4 This is a schematic diagram of the charge transport mechanism of carbon nitride / copper oxide composite materials;
[0044] Figure 5 This is a TEM image of the layered carbon nitride prepared in Example 1. Detailed Implementation
[0045] The technical solution of the present invention will be further described below with reference to specific embodiments. The scope of protection of the present invention is not limited to the following embodiments; these embodiments are listed for illustrative purposes only and do not limit the present invention in any way.
[0046] In the context of this specification, except where expressly stated, any matters or issues not mentioned herein are directly applicable to matters known in the art without modification. Furthermore, any embodiments described herein can be freely combined with one or more other embodiments described herein, and any resulting technical solutions or concepts shall be considered part of the original disclosure or original record of this invention, and should not be regarded as new content not disclosed or anticipated herein, unless those skilled in the art consider such combination to be clearly unreasonable.
[0047] This invention relates to the synthesis and carbon dioxide reduction application of a novel composite photocatalytic material of copper oxide or iron oxide and carbon nitride, belonging to the field of novel photocatalyst preparation technology. By directly growing copper oxide or iron oxide in situ hydrothermally onto carbon nitride, close contact between the two semiconductors can be achieved, thereby improving charge lifetime and promoting the photocatalytic process.
[0048] The carbon dioxide composite photocatalytic material is composed of one of copper oxide or iron oxide nanoparticles loaded on carbon nitride nanosheets, and the preferred loading amount of copper oxide or iron oxide on carbon nitride is 5wt%-30wt%.
[0049] The specific preparation process of the composite photocatalytic material of the present invention includes the following steps:
[0050] S1. Weigh out carbon and nitrogen-containing organic compounds, and obtain carbon nitride by calcining them at a programmed temperature and then cooling them to room temperature.
[0051] S2. The obtained carbon nitride is dispersed in water by ultrasonic treatment;
[0052] S3. Add the metal salt precursor and alkaline solution, mix thoroughly, and then transfer to a polytetrafluoroethylene-lined hydrothermal reactor for reaction.
[0053] S4. Centrifuge the product obtained in S3, wash it with water and ethanol respectively, and dry it.
[0054] S5. Calcination in a muffle furnace, followed by cooling to room temperature, yields the photocatalytic material.
[0055] As an improvement, in step S1, the carbon- and nitrogen-containing organic compounds used are melamine, dicyandiamide, and urea. The precursor is calcined at 520℃-600℃ for 2-4 hours.
[0056] As an improvement, in step S3, the metal salt precursor used is at least one of the chloride, nitrate, sulfate, and acetylacetonate of the corresponding metal.
[0057] As an improvement, in step S3, the alkaline solution used is an ammonia solution, a urea solution, a sodium hydroxide solution, or a potassium hydroxide solution.
[0058] As an improvement, in step S3, the hydrothermal reaction temperature is 120℃-150℃ and the time is 12 hours-48 hours.
[0059] As an improvement, in step S5, the calcination temperature is 200℃-300℃ and the time is 1 hour-2 hours.
[0060] Photocatalytic activity testing: The activity of the samples was tested using an online vacuum photocatalytic activity evaluation system.
[0061] The following embodiments further illustrate the present invention, but do not limit the present invention.
[0062] Photocatalytic carbon dioxide reduction applications
[0063] The obtained catalyst was used to simulate the photocatalytic reduction of CO2 under sunlight. Activity testing was conducted using an online vacuum photocatalytic reactor with a 300W xenon lamp as the light source. The reaction conditions were: 0.1g catalyst, 5mL water, three vacuum cycles (pressure <5KPa), followed by the introduction of high-purity CO2 gas to bring the pressure inside the reactor to 0.08MPa. After the reaction started, samples were taken every hour, and the products were analyzed using chromatography equipped with a flame ionization detector and a thermal conductivity detector. Quantification was performed using a pre-determined standard curve. The reaction mainly produced two products: CH4 and CO.
[0064] Example 1:
[0065] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 5℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 2g of copper nitrate was added, and after stirring for 1 hour, 15mL of 0.1mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 120℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, dried, and then calcined in a muffle furnace at 200℃ for 1 hour to obtain the carbon nitride / copper oxide composite material. (Appendix) Figure 1 This is an X-ray diffraction pattern of the carbon nitride / copper oxide composite material. It can be seen that the structure of the carbon nitride is well preserved after copper oxide growth. (Attached) Figure 2 This is the UV-Vis absorption spectrum of the carbon nitride / copper oxide composite material, showing that the composite material exhibits excellent light absorption properties. (Attached) Figure 3 It is the reaction between carbon nitride and copper oxide before and after ( Figure 3 a and Figure 3 b represents the fluorescence spectra before and after the carbon nitride and copper oxide composites, respectively. The results show that the fluorescence signal of carbon nitride significantly decreased after copper oxide growth, indicating that its photogenerated charge separation performance was improved. (Appendix) Figure 4 This is a schematic diagram of the charge transport mechanism of carbon nitride / copper oxide composite materials, conforming to the type II heterojunction mechanism. CBM and VBM represent the conduction band bottom and valence band top of the semiconductor, respectively. - and h + These correspond to photogenerated electrons and photogenerated holes, respectively. (See attached image.) Figure 5 The image shows a transmission electron microscope (TEM) image of carbon nitride obtained by programmed temperature calcination in Example 1. As can be seen from the image, carbon nitride has a layered structure.
[0066] Example 2:
[0067] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 5℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 3g of copper chloride was added, and after stirring for 1 hour, 10mL of 0.2mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, dried, and then calcined in a muffle furnace at 250℃ for 1 hour to obtain the carbon nitride / copper oxide composite material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 83.5μmol g, respectively. -1 h -1 and 7.6 μmol g -1 h -1 .
[0068] Example 3:
[0069] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 5℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 0.5g of copper nitrate was added, and after stirring for 1 hour, 10mL of 0.1mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, dried, and then calcined in a muffle furnace at 200℃ for 2 hours to obtain the carbon nitride / copper oxide composite material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 49.5μmol g, respectively. -1 h -1 and 4.1 μmol g -1 h -1 .
[0070] Example 4:
[0071] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 8℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 3g of ferric nitrate was added, and after stirring for 1 hour, 10mL of 0.2mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, washed 6 times with water and ethanol, dried, and then calcined in a muffle furnace at 200℃ for 1 hour to obtain the carbon nitride / iron oxide composite material. As shown in Appendix Table 1, its CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 30.9μmol g. -1 h -1 and 2.0 μmol g -1 h -1 .
[0072] Example 5:
[0073] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 10℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 1.5g of ferric chloride was added, and after stirring for 1 hour, 15mL of 0.1mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, washed 6 times with water and ethanol, dried, and then calcined in a muffle furnace at 200℃ for 1 hour to obtain the carbon nitride / iron oxide composite material. As shown in Appendix Table 1, its CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 55.1μmol g⁻¹. -1 h -1 and 2.0 μmol g -1 h -1 .
[0074] Example 6:
[0075] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 2℃ / min) - 600℃ (heating rate 8℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 1g of copper chloride and 1g of ferric chloride were added. After stirring for 1 hour, 10mL of 0.2mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, dried, and then calcined in a muffle furnace at 250℃ for 1 hour to obtain the carbon nitride / copper oxide composite material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 76.9 μmol g. -1 h -1 and 10.0 μmol g -1 h -1 .
[0076] Furthermore, comparative experiments confirmed that the synergistic effect of copper oxide or iron oxide with carbon nitride plays a crucial role in enhancing its reactivity, and minimizing the spatial distance between the two through in-situ hydrothermal synthesis is essential for maximizing this synergistic effect. Simultaneously, it was demonstrated that copper oxide or iron oxide with lower crystallinity is beneficial for improving photocatalytic activity. The specific scheme is as follows:
[0077] Comparative Example 1:
[0078] 20g of melamine was calcined using a heating program of room temperature - 550℃ (heating rate 2℃ / min) - 600℃ (heating rate 5℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 2g of copper nitrate and 50mL of water were weighed and stirred for 1 hour. Then, 15mL of 0.1mol / L ammonia solution was added dropwise. After stirring for another hour, the solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 120℃ for 24 hours. After the sample was naturally cooled to room temperature, it was washed six times with water and ethanol, and then vacuum dried at 40℃ to obtain copper oxide. 1g of carbon nitride and 0.25g of copper oxide were thoroughly ground and mixed to obtain the control material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 15.1μmol g⁻¹h⁻¹ and 1.5μmol g⁻¹, respectively. -1 h -1 .
[0079] Comparative Example 2:
[0080] 50g of melamine was weighed and calcined. The heating program was room temperature - 550℃ (heating rate 5℃ / min) - 600℃ (heating rate 10℃ / min). The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was weighed and ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 2g of copper nitrate was added, and after stirring for 1 hour, 15mL of 0.1mol / L ammonia solution was added dropwise. Stirring continued for 24 hours. After thoroughly washing with water to remove residual anions and drying, the mixture was calcined in a muffle furnace at 200℃ for 1 hour to obtain the control material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 4.2μmol g, respectively. -1 h -1 and 1.5 μmol g -1 h -1 .
[0081] Comparative Example 3
[0082] 50g of melamine was weighed and calcined at 550℃ for 4 hours. The resulting solid was ground to obtain the desired carbon nitride. 10g of carbon nitride was ultrasonically dispersed in 50mL of water (Kunshan Shumei Company, 40kHz) at room temperature. 3g of copper chloride was added, and after stirring for 1 hour, 10mL of 0.2mol / L ammonia solution was added dropwise. After stirring for another hour, the suspension was transferred to a polytetrafluoroethylene-lined reactor and reacted at 100℃ for 24 hours. After the sample was naturally cooled to room temperature, it was thoroughly washed with water to remove residual anions, dried, and then calcined in a muffle furnace at 250℃ for 1 hour to obtain the carbon nitride / copper oxide composite material. As shown in Appendix Table 1, the CO and CH4 generation rates in the photocatalytic carbon dioxide reduction test were 23.5μmol g, respectively. -1 h -1 and 7.6 μmol g -1 h -1 .
[0083] Table 1
[0084]
[0085]
[0086] *The stability of the photocatalyst was evaluated by a long-term activity test under continuous light irradiation. The activity change rate was calculated as: the total CO and CH4 generation rate after 24 hours of reaction / (initial total CO and CH4 generation rate) × 100%.
Claims
1. The application of a composite photocatalytic material in the reduction of carbon dioxide to CO and CH4, characterized in that, The composite photocatalytic material comprises metal oxide nanoparticles supported on carbon nitride; the carbon nitride has a two-dimensional nanosheet structure; the metal oxide nanoparticles are copper oxide nanoparticles and / or iron oxide nanoparticles. The content of the metal oxide is 5wt%-30wt%, and the content of carbon nitride is 70wt%-95wt%, wherein copper oxide is calculated as CuO, iron oxide as Fe2O3, and carbon nitride as C3N4. The preparation method of the photocatalytic material includes the following steps: S1. Preparation of carbon nitride, including: calcining a carbon-nitrogen-containing organic compound; the calcination process is to program the temperature from room temperature to a maximum calcination temperature, the maximum calcination temperature being 520℃-600℃, and the heating rate being 2-10℃ / min. S2. Disperse the carbon nitride prepared in step S1 in water to obtain dispersion A; S3. Add a soluble metal salt and an alkaline solution to dispersion A, mix thoroughly, and then carry out a hydrothermal reaction; the metal salt is a copper salt and / or an iron salt, the hydrothermal reaction temperature is 120℃-150℃, and the time is 12-48 hours. S4. Separate, wash and dry the product obtained in step S3 to obtain a solid product; S5. After calcining the solid product obtained in step S4, cool it to room temperature to obtain the photocatalytic material.
2. The application according to claim 1, characterized in that, The specific surface area of the carbon nitride is 4 m². 2 / g -10 m 2 / g.
3. The application according to claim 1, characterized in that, The carbon-nitrogen organic compound is one or more of melamine, dicyandiamide, and urea.
4. The application according to claim 1, characterized in that, In step S2, the weight ratio of water to carbon nitride is 5-0.5:
1.
5. The application according to claim 1, characterized in that, The metal salt is one or more of the chloride salt, nitrate salt, sulfate salt, and soluble organic salt of the corresponding metal.
6. The application according to claim 1, characterized in that, In step S3, the alkaline solution used is at least one of ammonia water, urea solution, sodium hydroxide solution, and potassium hydroxide solution; the concentration of the alkaline solution is 5wt%-50wt%.
7. The application according to claim 1, characterized in that, In step S5, the calcination temperature is 200℃-300℃, and the time is 1-2 hours.
Citation Information
Patent Citations
A heterojunction interface-doped composite photocatalyst and its preparation method
CN107308978B
Carbon nitride nanosheet-loaded titanium carbide quantum dot composite material and preparation method and application thereof
CN110013869A
Synthesis method and application of porous carbonitride / copper oxide nanorod composite material with visible light response
CN104907087A
Graphite-phase carbon nitride nanosheet-based composite photocatalytic material as well as preparation method and application thereof
CN109107601A