Low-e coated glass, laminated glass and vehicles

By setting a metal absorption layer on the side of the infrared reflective metal layer away from the glass substrate and optimizing the film structure, the problem of improving color and reflectivity in traditional low-emissivity coated glass in laminated glass is solved, achieving low cost, low transmittance and high infrared reflectivity, and improving the thermal insulation performance of laminated glass.

CN117682773BActive Publication Date: 2026-11-20FUJIAN WANDA AUTOMOBILE GLASS IND
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311420012.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-20
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

When traditional low-emissivity coated glass is applied to laminated glass, the heat insulation effect decreases as visible light transmittance decreases and color and reflectivity increase. Furthermore, the use of colored PVB with low light transmittance increases production costs.

Method used

A low-emissivity coated glass is designed by setting a metal absorption layer on the side of the infrared reflective metal layer away from the glass substrate, and optimizing the thickness and material of each film layer to form a structure with at least two infrared reflective metal layers and one metal absorption layer, thus avoiding the use of a low-transmittance PVB adhesive layer.

Benefits of technology

Without increasing costs, it achieves low visible light transmittance, high infrared reflectance, and good appearance color, thus improving the heat insulation effect of laminated glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117682773B_ABST
    Figure CN117682773B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of low emissivity coated glass, laminated glass and vehicle.The above-mentioned low emissivity coated glass includes first glass substrate and the coated layer of at least one surface of first glass substrate, at least two infrared reflective metal layers and at least one metal absorption layer are arranged in the coated layer, the metal absorption layer is arranged on the side of all infrared reflective metal layers away from the first glass substrate;Wherein, the geometric thickness of the metal absorption layer is greater than or equal to 7nm.The above-mentioned low emissivity coated glass is applied in laminated glass, can make laminated glass have low visible light transmittance, higher infrared reflective function and better appearance color while reducing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional glass, and in particular to a low-emissivity coated glass, laminated glass, and vehicles. Background Technology

[0002] Currently, sunroofs used in vehicles achieve heat insulation by coating the inner surface of the outer glass with an infrared reflective film containing multiple layers of metallic silver. However, sunroofs typically require low visible light transmittance, usually less than 20% or 10%. To meet these transmittance requirements, low-transmittance tinted PVB is generally used as the interlayer in the laminated glass. However, this low-transmittance tinted PVB is usually expensive, increasing the production cost of laminated glass to some extent.

[0003] In traditional technology, transparent PVB is used as the bonding layer of laminated glass to reduce costs, and various low-emissivity coated glasses have been disclosed. However, when traditional low-emissivity coated glass is used in laminated glass, as the visible light transmittance further decreases, it usually brings unfavorable color and increased reflectivity to the laminated glass, reducing the heat insulation effect of the laminated glass. Summary of the Invention

[0004] Based on this, some embodiments of the present invention provide a low-emissivity coated glass, which, when applied in laminated glass, enables the laminated glass to reduce costs while having low visible light transmittance, high infrared reflection, and good appearance color.

[0005] Furthermore, other embodiments of the present invention also provide a laminated glass comprising the aforementioned low-emissivity coated glass and a vehicle.

[0006] A low-emissivity coated glass includes a first glass substrate and a coating layer disposed on at least one surface of the first glass substrate. The coating layer includes at least two infrared-reflecting metal layers and at least one metal-absorbing layer stacked together. The metal-absorbing layer is disposed on the side of all infrared-reflecting metal layers away from the first glass substrate.

[0007] The geometric thickness of the metal absorption layer is ≥7nm.

[0008] In some embodiments, the coating layer includes an inner dielectric layer, a first infrared reflective metal layer, a first intermediate dielectric layer, a second infrared reflective metal layer, a second intermediate dielectric layer, a metal absorption layer, and an outer dielectric layer stacked sequentially, wherein the inner dielectric layer is closer to the first glass substrate than the outer dielectric layer.

[0009] In some embodiments, the metal absorbing layer satisfies one or more of the following conditions:

[0010] (1) The material of the metal absorption layer includes one or more alloys of W, Ni, Cr, Ti, Nb, Mo, Si and Zr;

[0011] Optionally, the material of the metal absorption layer includes one of W, Ti, and NiCr;

[0012] (2) The total geometric thickness of the metal absorption layer disposed on the side of all infrared reflective metal layers away from the first glass substrate is ≥7nm, and the total geometric thickness of the metal absorption layer is ≤50nm.

[0013] In some embodiments, the metal absorbing layer includes a first metal layer close to the first glass substrate and a second metal layer further away from the first glass substrate than the first metal layer, wherein the first metal layer and the second metal layer satisfy one or more of the following conditions:

[0014] (1) The geometric thickness of the first metal layer is ≥2nm;

[0015] (2) The geometric thickness of the second metal layer is ≥5nm;

[0016] (3) A third intermediate dielectric layer is further provided between the first metal layer and the second metal layer;

[0017] Optionally, the geometric thickness of the third intermediate dielectric layer is 20 nm to 80 nm;

[0018] Optionally, the material of the third intermediate dielectric layer includes an oxide of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W, and Bi, or one or more nitrides and oxynitrides selected from at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb, and Ta.

[0019] In some embodiments, the infrared-reflective metal layer satisfies one or more of the following conditions:

[0020] (1) The material of each infrared reflective metal layer independently includes any one or more alloys of Ag, Au, Cu, Al, Pt, Pd, Mo and In;

[0021] Optionally, the material of each of the infrared reflective metal layers includes Ag;

[0022] (2) The geometric thickness of each infrared reflective metal layer is independently 5nm~20nm.

[0023] In some embodiments, the inner dielectric layer satisfies one or more of the following conditions:

[0024] (1) The material of the inner dielectric layer includes one or more of the oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more of the nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

[0025] (2) The geometric thickness of the inner dielectric layer is 15nm~50nm.

[0026] In some embodiments, the first intermediate dielectric layer satisfies one or more of the following conditions:

[0027] (1) The geometric thickness of the first intermediate dielectric layer is 40 nm to 100 nm;

[0028] (2) The material of the first intermediate dielectric layer includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

[0029] In some embodiments, the second intermediate dielectric layer satisfies one or more of the following conditions:

[0030] (1) The material of the second intermediate dielectric layer includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

[0031] Optionally, the material of the second intermediate dielectric layer includes SiN. x ;

[0032] (2) The geometric thickness of the second intermediate dielectric layer is 10nm~100nm.

[0033] In some embodiments, the outer dielectric layer satisfies one or more of the following conditions:

[0034] (1) The geometric thickness of the outer dielectric layer is ≥5nm;

[0035] (2) The material of the outer dielectric layer includes one or more of the nitrides and oxides of at least one of the elements selected from Si, Al, Zr, Ti and B;

[0036] Optionally, the material of the outer dielectric layer includes SiN.x .

[0037] In some embodiments, the coating layer further includes a first barrier layer and / or a second barrier layer, wherein the first barrier layer is disposed between the first infrared reflective metal layer and the first intermediate dielectric layer, the geometric thickness of the first barrier layer is 0.5 nm to 10 nm, and the material of the first barrier layer includes one or more of the metals, alloys, oxides and nitrides of at least one element selected from Ni, Cr, Ti, Zn, Nb, Hf, Zr and Al;

[0038] The second barrier layer is disposed between the second infrared reflective metal layer and the second intermediate dielectric layer. The geometric thickness of the second barrier layer is 0.5 nm to 10 nm. The material of the second barrier layer includes one or more of the metals, alloys, oxides and nitrides of at least one element, such as Ni, Cr, Ti, Zn, Nb, Hf, Zr and Al.

[0039] A laminated glass comprising the aforementioned low-emissivity coated glass, an adhesive layer, and a second glass substrate, wherein the adhesive layer is disposed between the coated layer and the second glass substrate and is located on the side of the coated layer away from the first glass substrate.

[0040] In some embodiments, the visible light transmittance of the first glass substrate is ≥70%, the visible light transmittance of the second glass substrate is ≤50%, and the visible light transmittance of the adhesive layer is ≥70%.

[0041] In some embodiments, the visible light transmittance of the laminated glass is ≤10%.

[0042] In some embodiments, the visible light reflectance of the laminated glass is ≤20%.

[0043] In some embodiments, the total solar transmittance of the laminated glass is ≤25%.

[0044] In some embodiments, the reflected color of the laminated glass surface has a color component L value of 0~60, a color component a value of -5~0, and a color component b value of -15~0 in the Lab color space.

[0045] A vehicle comprising the aforementioned laminated glass.

[0046] The aforementioned low-emissivity coated glass includes a first glass substrate and a coating layer disposed on at least one surface of the first glass substrate. The coating layer includes at least two infrared reflective metal layers and at least one metal absorbing layer stacked together. By disposing the metal absorbing layer on the side away from the first glass substrate from all infrared reflective metal layers and adjusting the thickness of the metal absorbing layer, the laminated glass prepared from the aforementioned low-emissivity coated glass still meets the requirements of low visible light transmittance, visible light reflectance, total solar energy transmittance, and aesthetically pleasing color indicators without using a low-transmittance PVB bonding layer. Attached Figure Description

[0047] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0048] Figure 1 A schematic diagram of a low-emissivity coated glass provided in some embodiments of the present invention;

[0049] Figure 2 This is a schematic diagram of another structure of low-emissivity coated glass provided in some embodiments of the present invention;

[0050] Figure 3 This is a schematic diagram of a structure of laminated glass provided in some embodiments of the present invention;

[0051] Figure 4 This is a schematic diagram of another structure of laminated glass provided in some embodiments of the present invention.

[0052] Explanation of reference numerals in the attached figures:

[0053] Laminated glass 10, low-emissivity coated glass 100, first glass substrate 101, inner dielectric layer 102, first infrared reflective metal layer 103, first barrier layer 104, first intermediate dielectric layer 105, second infrared reflective metal layer 106, second barrier layer 107, second intermediate dielectric layer 108, metal absorbing layer 109, first metal layer 1092, second metal layer 1094, outer dielectric layer 110, third intermediate dielectric layer 111, adhesive layer 200, second glass substrate 300. Detailed Implementation

[0054] To facilitate understanding of the present invention, a more comprehensive description of the invention will be provided below in conjunction with specific embodiments. Preferred embodiments of the invention are given in the specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the present invention.

[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0056] Unless otherwise stated or in case of contradiction, the terms or phrases used in this invention shall have the following meanings:

[0057] The term "and / or" as used in this invention includes any and all combinations of one or more of the associated listed items.

[0058] In this invention, terms such as "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features.

[0059] In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0060] When a numerical range is disclosed in this invention, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Further, when the range refers to an integer, it includes every integer between the minimum and maximum values ​​of the range. Moreover, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed in this invention should be understood to include any and all subranges to which they are incorporated.

[0061] The names of the various film materials mentioned in this invention are not limited to their chemical formulas; they may refer to the main elemental components contained in each film layer, or the abbreviations of the main components, such as "SiN". x "It can be Si3N4, ZnSnO" x "It can be ZnSnO4, etc., but this application does not limit it."

[0062] A first aspect of the present invention provides a low-emissivity coated glass with low visible light transmittance and high infrared reflectance, comprising a first glass substrate and a coating layer disposed on at least one surface of the first glass substrate, the coating layer comprising at least two infrared reflective metal layers and at least one metal absorbing layer stacked thereon, the metal absorbing layer being disposed on the side of all infrared reflective metal layers away from the first glass substrate.

[0063] The geometric thickness of the metal absorption layer is ≥7nm.

[0064] It is understood that, unless otherwise specified, in this article, geometric thickness refers to the physical thickness of the thin film layer, and the product of geometric thickness and the refractive index of the thin film layer is called optical thickness.

[0065] It is understood that there can be two or three infrared reflective metal layers, and the metal absorption layer is disposed on the side of all infrared reflective metal layers away from the first glass substrate.

[0066] In some embodiments, there are two infrared reflective metal layers, and a metal absorption layer is disposed on the side of the two infrared reflective metal layers away from the first glass substrate.

[0067] In some embodiments, the geometric thickness of the metal absorbing layer is ≥7 nm. For example, the geometric thickness of the metal absorbing layer may be, but is not limited to, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, or any range of two of these values. Preferably, the geometric thickness of the metal absorbing layer is ≥10 nm. Further, the total geometric thickness of the metal absorbing layer is ≤50 nm.

[0068] In some embodiments, the material of the metal absorbing layer includes one or more alloys selected from W, Ni, Cr, Ti, Nb, Mo, Si, and Zr. In some embodiments, the material of the metal absorbing layer includes one of W, Ti, and NiCr.

[0069] In some embodiments, the metal absorbing layer is a single-layer structure. In other embodiments, the metal absorbing layer is a double-layer structure, comprising a first metal layer close to the first glass substrate and a second metal layer further away from the first glass substrate than the first metal layer. The geometric thickness of the first metal layer is ≥2 nm, and the geometric thickness of the second metal layer is ≥5 nm. An intermediate dielectric layer is also provided between the first and second metal layers. Setting the metal absorbing layer as a double-layer structure can further reduce the visible light transmittance of the coated glass while maintaining high infrared reflectivity.

[0070] In some embodiments, the material of each infrared reflective metal layer independently includes one or more alloys selected from Ag, Au, Cu, Al, Pt, Pd, Mo, and In. It is understood that the materials of each infrared reflective metal layer may be the same or different; preferably, the materials of each infrared reflective metal layer are the same.

[0071] In one embodiment, the material of each infrared reflective metal layer includes Ag.

[0072] In some embodiments, the geometric thickness of each infrared reflective metal layer is independently 5 nm to 20 nm. For example, the geometric thickness of each infrared reflective metal layer may be, but is not limited to, 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm, or any combination of these values.

[0073] In some embodiments, please refer to Figure 1 The low-emissivity coated glass 100 includes a first glass substrate 101 and a coating layer disposed on at least one surface of the first glass substrate 101. The coating layer includes an inner dielectric layer 102, a first infrared reflective metal layer 103, a first intermediate dielectric layer 105, a second infrared reflective metal layer 106, a second intermediate dielectric layer 108, a metal absorption layer 109, and an outer dielectric layer 110, which are stacked sequentially.

[0074] The geometric thickness of the metal absorption layer 109 is ≥7nm.

[0075] It is understood that in this article, the stacking arrangement only indicates the stacking order between the layers, but is not limited to the layers mentioned above. Other layers may also be stacked between the layers.

[0076] In some embodiments, the geometric thickness of the inner dielectric layer 102 is 15 nm to 50 nm. For example, the geometric thickness of the inner dielectric layer 102 may be, but is not limited to, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, or any combination of these values.

[0077] In some embodiments, the material of the inner dielectric layer 102 includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

[0078] In some embodiments, the material of the inner dielectric layer 102 includes ZnSnO. x SiN xAnd one or more of AZO (aluminum-doped zinc oxide). Further, in some embodiments, the inner dielectric layer 102 comprises ZnSnO. x or SiN x The first inner layer is composed of a first inner layer and a second inner layer composed of AZO, with the first inner layer being closer to the first glass substrate than the second inner layer.

[0079] Furthermore, the geometric thickness of the first inner layer is 15nm to 35nm, and the geometric thickness of the second inner layer is 10nm to 25nm. For example, the geometric thickness of the first inner layer can be, but is not limited to, 15nm, 16nm, 18nm, 20nm, 22nm, 24nm, 25nm, 26nm, 28nm, 30nm, 32nm, 34nm, 35nm, or any combination of these values. The geometric thickness of the second inner layer can be, but is not limited to, 10nm, 12nm, 14nm, 15nm, 16nm, 18nm, 20nm, 22nm, 24nm, 25nm, or any combination of these values. It is understood that only one structure of the inner dielectric layer 102 has been given above, but the inner dielectric layer 102 is not limited to the structure described above.

[0080] In some embodiments, the material of the inner dielectric layer 102 includes AZO. Materials like AZO have the function of isolating oxygen, which can protect the infrared reflective metal layer such as the silver layer and increase the adhesion between the film layers. In addition, AZO can provide good structural properties that help the growth of the infrared reflective metal layer such as the silver layer.

[0081] In some embodiments, the material of the first infrared reflective metal layer 103 includes one or more alloys of Ag, Au, Cu, Al, Pt, Pd, Mo, and In. In one embodiment, the material of the first infrared reflective metal layer 103 includes Ag.

[0082] In some embodiments, the geometric thickness of the first infrared reflective metal layer 103 is 5 nm to 20 nm. For example, the geometric thickness of the first infrared reflective metal layer 103 may be, but is not limited to, 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm, or any combination of these values.

[0083] In some embodiments, the geometric thickness of the first intermediate dielectric layer 105 is 40 nm to 100 nm. For example, the geometric thickness of the first intermediate dielectric layer 105 may be, but is not limited to, 40 nm, 45 nm, 50 nm, 52 nm, 54 nm, 55 nm, 56 nm, 58 nm, 60 nm, 62 nm, 64 nm, 65 nm, 66 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, or any combination of these values.

[0084] In some embodiments, the material of the first intermediate dielectric layer 105 includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

[0085] In some embodiments, the material of the first intermediate dielectric layer 105 includes ZnSnO. x SiN x And one or more of AZO. In some embodiments, the first intermediate dielectric layer 105 comprises ZnSnO. x or SiN x The system comprises a first intermediate layer and a second intermediate layer composed of AZO, with the first intermediate layer positioned closer to the first glass substrate than the second intermediate layer. The geometric thickness of the first intermediate layer is 40 nm to 60 nm, and the geometric thickness of the second intermediate layer is 10 nm to 30 nm. For example, the geometric thickness of the first intermediate layer can be, but is not limited to, 40 nm, 42 nm, 44 nm, 45 nm, 46 nm, 48 nm, 50 nm, 52 nm, 54 nm, 55 nm, 56 nm, 58 nm, 60 nm, or any combination of these values. The geometric thickness of the second intermediate layer can be, but is not limited to, 10 nm, 12 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm, 22 nm, 24 nm, 25 nm, 26 nm, 28 nm, 30 nm, or any combination of these values.

[0086] It is understood that the above only presents one structure of the first intermediate dielectric layer 105, but is not limited to this.

[0087] In some embodiments, the material of the second infrared reflective metal layer 106 includes one or more alloys selected from Ag, Au, Cu, Al, Pt, Pd, Mo, and In. In one embodiment, the material of the second infrared reflective metal layer 106 includes Ag.

[0088] In some embodiments, the geometric thickness of the second infrared reflective metal layer 106 is 5 nm to 20 nm. For example, the geometric thickness of the second infrared reflective metal layer 106 may be, but is not limited to, 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm, or any combination of these values.

[0089] It is understood that the material of the second infrared reflective metal layer 106 can be the same as or different from the material of the first infrared reflective metal layer 103. Preferably, the material of the second infrared reflective metal layer 106 is the same as the material of the first infrared reflective metal layer 103.

[0090] In some embodiments, the geometric thickness of the second intermediate dielectric layer 108 is 10 nm to 100 nm. For example, the geometric thickness of the second intermediate dielectric layer 108 may be, but is not limited to, 15 mm, 20 nm, 30 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 62 mm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, or any combination of these values.

[0091] Preferably, in Figure 1 In this structure, the metal absorption layer 109 is a single-layer structure, and the geometric thickness of the second intermediate dielectric layer 108 is 20nm~100nm, more preferably 30nm~80nm.

[0092] In some embodiments, the material of the second intermediate dielectric layer 108 includes an oxide of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W, and Bi, or one or more nitrides and oxynitrides selected from Si, Al, Zr, Ti, Y, Hf, Nb, and Ta. In some embodiments, the material of the second intermediate dielectric layer 108 includes SiN x .

[0093] In some embodiments, the material of the metal absorbing layer 109 includes one or more alloys selected from W, Ni, Cr, Ti, Nb, Mo, Si, and Zr. In some embodiments, the material of the metal absorbing layer 109 includes one of W, Ti, and NiCr.

[0094] In some embodiments, the geometric thickness of the metal absorption layer 109 is ≥7 nm. For example, the geometric thickness of the metal absorption layer 109 may be, but is not limited to, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 22 nm, 25 nm, 30 nm, 40 nm, 50 nm, or any range of two of these values. Preferably, the geometric thickness of the metal absorption layer 109 is ≥10 nm. Further, the total geometric thickness of the metal absorption layer 109 is ≤50 nm.

[0095] In some embodiments, the outer dielectric layer 110 is located furthest from the surface of the first glass substrate 101, and the material of the outer dielectric layer 110 includes one or more of the nitrides and oxides of at least one element selected from Si, Al, Zr, Ti, and B. In some embodiments, the material of the outer dielectric layer 110 includes SiN. x .

[0096] In some embodiments, the geometric thickness of the outer dielectric layer 110 is ≥5 nm. For example, the geometric thickness of the outer dielectric layer 110 may be, but is not limited to, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, or any combination of these values.

[0097] In some embodiments, the coating layer further includes a first barrier layer 104 and / or a second barrier layer 107.

[0098] The first barrier layer 104 is located between the first infrared reflective metal layer 103 and the first intermediate dielectric layer 105. The geometric thickness of the first barrier layer 104 is 0.5nm~10nm. The material of the first barrier layer 104 includes one or more of the metals, alloys, oxides and nitrides of at least one element selected from Ni, Cr, Ti, Zn, Nb, Hf, Zr and Al.

[0099] It is understood that oxides include both complete oxides and incomplete oxides. Similarly, nitrides include both complete nitrides and incomplete nitrides. In some embodiments, the material of the first barrier layer 104 includes AZO.

[0100] The second barrier layer 107 is located between the second infrared reflective metal layer 106 and the second intermediate dielectric layer 108. The geometric thickness of the second barrier layer 107 is 0.5 nm to 10 nm. The material of the second barrier layer 107 includes one or more of the metals, alloys, oxides, and nitrides of at least one element, such as Ni, Cr, Ti, Zn, Nb, Hf, Zr, and Al. In some embodiments, the material of the second barrier layer 107 includes AZO.

[0101] Optionally, the geometric thickness of the first barrier layer 104 may be, but is not limited to, 0.5nm, 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, or any combination of these values.

[0102] Optionally, the geometric thickness of the second barrier layer 107 may be, but is not limited to, 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any combination of these values.

[0103] exist Figure 1 In this embodiment, the metal absorption layer 109 has a single-layer structure. In other embodiments, the metal absorption layer 109 has a double-layer structure; please refer to [link to relevant documentation]. Figure 2 The metal absorption layer 109 includes a first metal layer 1092 and a second metal layer 1094, and a third intermediate dielectric layer 111 is further provided between the first metal layer 1092 and the second metal layer 1094. Specifically, in Figure 2 In the low-emissivity coated glass 100, there are a first glass substrate 101 and a coating layer disposed on at least one surface of the first glass substrate 101. The coating layer includes the following layers stacked in sequence: an inner dielectric layer 102, a first infrared reflective metal layer 103, a first intermediate dielectric layer 105, a second infrared reflective metal layer 106, a second intermediate dielectric layer 108, a first metal absorption layer 109, a third intermediate dielectric layer 111, a second metal absorption layer 109, and an outer dielectric layer 110.

[0104] Specifically, the material of the first metal layer 1092 includes one or more alloys selected from W, Ni, Cr, Ti, Nb, Mo, Si, and Zr. In some embodiments, the material of the first metal layer 1092 includes W, Ti, or NiCr.

[0105] In some embodiments, the geometric thickness of the first metal layer 1092 is ≥2nm, and the first metal layer 1092 is located above all infrared reflective metal layers, i.e., between the second infrared reflective metal layer 106 and the outer dielectric layer 110. For example, the geometric thickness of the first metal layer 1092 may be, but is not limited to, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 12nm, 14nm, 15nm, 18nm, 20nm, or any combination of these values. Optionally, the geometric thickness of the first metal layer 1092 may be 2nm~20nm, 2nm~15nm, 2nm~12nm, 2nm~10nm, 4nm~20nm, 4nm~15nm, 4nm~12nm, 4nm~10nm, etc.

[0106] In some embodiments, the geometric thickness of the third intermediate dielectric layer 111 is 20 nm to 80 nm. For example, the geometric thickness of the third intermediate dielectric layer 111 may be, but is not limited to, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, or any combination of these values.

[0107] In some embodiments, the material of the third intermediate dielectric layer 111 includes an oxide of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W, and Bi, or one or more nitrides and oxynitrides selected from Si, Al, Zr, Ti, Y, Hf, Nb, and Ta. Optionally, the material of the third intermediate dielectric layer 111 includes SiN x .

[0108] In some embodiments, the material of the second metal layer 1094 includes one or more alloys selected from W, Ni, Cr, Ti, Nb, Mo, Si, and Zr. In one embodiment, the material of the second metal layer 1094 includes one of W, Ti, and NiCr.

[0109] In some embodiments, the geometric thickness of the second metal layer 1094 is ≥5 nm. For example, the geometric thickness of the second metal layer 1094 may be, but is not limited to, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, or any combination of these values. Preferably, the geometric thickness of the second metal layer 1094 is 7 nm to 20 nm.

[0110] By setting the metal absorption layer 109 as a double-layer structure, the visible light transmittance of the coated glass can be further reduced while ensuring high infrared reflectivity.

[0111] exist Figure 2 In the middle, the inner dielectric layer 102, the first infrared reflective metal layer 103, the second infrared reflective metal layer 106, the first intermediate dielectric layer 105, the second intermediate dielectric layer 108, the outer dielectric layer 110, the first barrier layer 104, and the second barrier layer 107 are the same as those described above, and will not be repeated here.

[0112] Preferably, in Figure 2 In the process, the metal absorption layer 109 has a two-layer structure, and the geometric thickness of the second intermediate dielectric layer 108 is preferably 10nm~40nm, and more preferably 15nm~30nm.

[0113] A conventional technique discloses a low-emissivity, high infrared reflectance coated glass. In this coated glass, the barrier layer that directly contacts the infrared-reflecting Ag layer is a NiCr metal absorbing layer with certain light absorption properties, i.e., a NiCr metal with SiN... x / NiCr / Ag / NiCr / SiN x / NiCr / Ag / NiCr / SiN x The low-emissivity coating of the stacked layers; and the visible light transmittance is reduced by adjusting the geometric thickness of the NiCr layer. The visible light transmittance is generally 50%~60%. However, when this technology is used in laminated glass, the following problems exist: (1) When the visible light transmittance is further reduced to ≤30%, the increase in the geometric thickness of the NiCr layer may cause unfavorable color and reflectivity of the laminated glass; (2) When the NiCr layer is in contact with the infrared reflective metal layer Ag layer, the further increase in the geometric thickness of the NiCr layer will directly affect the infrared reflectivity of the low-e film layer and reduce the heat insulation effect of the laminated glass; (3) With the increase in the geometric thickness of the NiCr layer, after the glass is heat-treated at 500℃~650℃, the film layer will produce high haze and other problems.

[0114] Therefore, in conventional technologies, nickel-chromium is used as a contact layer for the Ag layer to improve chemical, mechanical, and environmental durability (compared to using a zinc oxide lower contact layer under silver and / or a highly oxidized nickel-chromium upper contact layer over silver), while the nickel-chromium layer can also be used as a metal absorbing layer.

[0115] In this application, it was found that placing the metal absorption layer above the double silver layer can actually achieve better physicochemical parameters and obtain unexpected technical effects. Specifically, in some embodiments of the present invention, the low-emissivity coated glass 100 places the metal absorption layer 109 on the side surface of all infrared reflective metal layers away from the first glass substrate 101, and designs and optimizes each film layer so that, without using a low-transmittance PVB adhesive layer, the laminated glass prepared from the above-mentioned low-emissivity coated glass 100 still meets the requirements of low visible light transmittance, visible light reflectance, total solar energy transmittance, and aesthetic color index.

[0116] A second aspect of the present invention provides a laminated glass comprising the aforementioned low-emissivity coated glass, an adhesive layer, and a second glass substrate, wherein the adhesive layer is disposed between the coated layer and the second glass substrate and is located on the side surface of the coated layer away from the first glass substrate.

[0117] Please see Figure 3 In some embodiments, the laminated glass 10 includes a low-emissivity coated glass 100, an adhesive layer, and a second glass substrate 300. An adhesive layer 200 is disposed between the coated layer and the second glass substrate 300, and is located on the surface of the coated layer away from the first glass substrate 101. The low-emissivity coated glass 100 includes a first glass substrate 101 and a coated layer disposed on at least one surface of the first glass substrate 101. The coated layer includes, in sequence, an inner dielectric layer 102, a first infrared-reflecting metal layer 103, a first barrier layer 104, a first intermediate dielectric layer 105, a second infrared-reflecting metal layer 106, a second barrier layer 107, a second intermediate dielectric layer 108, a metal-absorbing layer 109, and an outer dielectric layer 110.

[0118] Please see Figure 4 In some other embodiments, the laminated glass 10 includes a low-emissivity coated glass 100, an adhesive layer, and a second glass substrate 300. An adhesive layer 200 is disposed between the coated layer and the second glass substrate 300, and is located on the surface of the coated layer away from the first glass substrate 101. The low-emissivity coated glass 100 includes a first glass substrate 101 and a coated layer disposed on at least one surface of the first glass substrate 101. The coated layer includes, in sequence, an inner dielectric layer 102, a first infrared-reflecting metal layer 103, a first barrier layer 104, a first intermediate dielectric layer 105, a second infrared-reflecting metal layer 106, a second barrier layer 107, a second intermediate dielectric layer 108, a first metal layer 1092, a third intermediate dielectric layer 111, a second metal layer 1094, and an outer dielectric layer 110.

[0119] In some embodiments, the first glass substrate 101 and / or the second glass substrate 300 are transparent glass. The visible light transmittance of the transparent glass is ≥70%. For example, the transparent glass may be, but is not limited to, clear glass.

[0120] In other embodiments, the first glass substrate 101 and / or the second glass substrate 300 are tinted glass, and the visible light transmittance of the tinted glass is ≤50%. For example, the tinted glass may be, but is not limited to, gray glass.

[0121] In some embodiments, the first glass substrate 101 is transparent glass, and the second glass substrate 300 is tinted glass. Specifically, the visible light transmittance of the first glass substrate 101 is ≥70%, and the visible light transmittance of the second glass substrate 300 is ≤50%.

[0122] In some embodiments, the adhesive layer 200 may be a colorless and transparent or colored low-transmittance polymer layer. Specifically, the material of the adhesive layer 200 includes one or more of PVB (polyvinyl butyral), PU (polyurethane), EVA (ethylene-ethyl acetate copolymer), and SGP (ionic interlayer).

[0123] In some embodiments, the visible light transmittance of the adhesive layer 200 is ≤30%. For example, the adhesive layer 200 comprises a gray PVB adhesive layer. The visible light transmittance of the gray PVB adhesive layer is 10±2%. In other embodiments, the visible light transmittance of the adhesive layer 200 is ≥70%. For example, the adhesive layer 200 comprises a transparent PVB adhesive layer. The visible light transmittance of the transparent PVB adhesive layer is >90%.

[0124] Preferably, the visible light transmittance of the adhesive layer 200 is ≥70%. High visible light transmittance of the adhesive layer 200 helps to reduce costs.

[0125] In some embodiments, the visible light transmittance of the first glass substrate 101 is ≥70%, the visible light transmittance of the second glass substrate 300 is ≤50%, and the visible light transmittance of the adhesive layer 200 is ≥70%.

[0126] In some embodiments, the visible light transmittance of the laminated glass 10 is ≤10%. For example, the visible light transmittance of the laminated glass 10 may be, but is not limited to, 10%, 9.5%, 9%, 8.5%, 8%, 7.5%, 7%, 6.5%, 6%, or any combination of these values.

[0127] In some embodiments, the visible light reflectance of the laminated glass 10 is ≤20%. For example, the visible light reflectance of the laminated glass 10 may be, but is not limited to, 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, or any combination of these values. Preferably, the visible light reflectance of the laminated glass 10 is ≤15%.

[0128] In some embodiments, the total solar transmittance of the laminated glass 10 is ≤25%. For example, the total solar transmittance of the laminated glass 10 may be, but is not limited to, 25%, 24%, 23%, 22%, 21%, 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, or any combination of these values. Preferably, the total solar transmittance of the laminated glass 10 is ≤20%.

[0129] In some embodiments, the reflected color of the laminated glass surface is described using the CIELab color space, where dimension L represents brightness, a and b represent opposite color dimensions, color component a represents the component from green to red, and color component b represents the component from blue to yellow. In this application, the color component L value is 0~60, the color component a value is -5~0, and the color component b value is -15~0. For example, the color component L value can be, but is not limited to, 0, 5, 10, 15, 20, 25, 30, 32, 34, 35, 36, 38, 40, 42, 44, 45, 46, 48, 50, 55, 60, or any two of these values. The color component a value can be, but is not limited to, -5, -4, -3, -2, -1, 0, or any two of these values. The color component b value can be, but is not limited to, -15, -12, -10, -8, -6, -5, -4, -2, 0, or any combination of these values. In addition, in some specific embodiments, the color component L value is 30 to 50, the color component a value is -4 to -1, and the color component b value is -13 to -5.

[0130] It is understood that in some embodiments, when the laminated glass 10 is used as automotive window glass, the first glass substrate 101 refers to the glass substrate of the laminated glass 10 adjacent to the air surface outside the vehicle, also known as the outer glass substrate, and the second glass substrate 300 refers to the glass substrate of the laminated glass 10 adjacent to the air surface inside the vehicle, also known as the inner glass substrate. The "outer surface of the glass substrate" refers to the interface of the laminated glass 10 in contact with the air surface, and the "inner surface of the glass substrate" refers to the interface of the laminated glass 10 in contact with the adhesive layer 200.

[0131] The aforementioned laminated glass 10, even when using a lower-cost transparent adhesive layer 200, still meets the requirements for lower visible light transmittance, visible light reflectance, total solar energy transmittance, and aesthetically pleasing color indicators.

[0132] A third aspect of the present invention provides a vehicle comprising the aforementioned laminated glass.

[0133] It is understandable that laminated glass can be used as sunroof glass, side window glass, etc. in vehicles.

[0134] It is understandable that other components in the vehicle can be those commonly used in this field, and will not be described in detail here.

[0135] To make the objectives and advantages of the present invention clearer, the low-emissivity coated glass and its effects of the present invention are further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and should not be used to limit the present invention. Unless otherwise specified, the following embodiments do not include components other than unavoidable impurities. Unless otherwise specified, the drugs and instruments used in the embodiments are conventional choices in the art. Experimental methods in the embodiments that do not specify specific conditions are implemented according to conventional conditions, such as those described in literature, books, or methods recommended by the manufacturer.

[0136] Comparative Example 1

[0137] Comparative Example 1 provides a laminated glass comprising an outer glass substrate and an inner glass substrate, wherein both the outer and inner glass substrates are made of clear glass with a geometric thickness of 2.1 mm. The inner surface of the outer glass substrate is coated with an infrared-reflective low-emissivity film by magnetron sputtering, and the film comprises, sequentially stacked ZnSnO in the direction from the inner surface near the outer glass substrate to the inner surface away from the outer glass substrate. x 30nm / AZO 10nm / Ag 10nm / AZO 10nm / ZnSnO x 55nm / AZO 10nm / Ag11nm / AZO 10nm / ZnSnO x 15nm / SiN x 10nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a gray PVB adhesive layer with a transmittance of 10±2%.

[0138] Comparative Example 2

[0139] Comparative Example 2 provides a laminated glass comprising an outer glass substrate and an inner glass substrate, wherein both the outer and inner glass substrates are made of clear glass with a geometric thickness of 2.1 mm. The inner surface of the outer glass substrate is coated with an infrared-reflective low-emissivity film by magnetron sputtering, and the film comprises, sequentially stacked layers of: SiN... x 20nm / AZO 10nm / Ag 11nm / NiCr 8nm / SiN x 65nm / AZO 20nm / Ag 10nm / NiCr 5nm / AZO 12nm / SiN x22nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0140] Comparative Example 3

[0141] Comparative Example 3 provides a laminated glass comprising an outer glass substrate and an inner glass substrate, wherein both the outer and inner glass substrates are made of clear glass with a geometric thickness of 2.1 mm. The inner surface of the outer glass substrate is coated with an infrared-reflective low-emissivity film using magnetron sputtering, and the film comprises, sequentially stacked layers of: SiN... x 15nm / AZO 10nm / Ag 12nm / NiCr 12nm / SiN x 65nm / AZO 20nm / Ag 11nm / NiCr 12nm / AZO 12nm / SiN x 22nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0142] Comparative Example 4

[0143] Comparative Example 4 provides a laminated glass comprising an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25% to 30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked layers of: SiN... x 20nm / AZO 10nm / Ag11nm / NiCr 8nm / SiN x 65nm / AZO 20nm / Ag 10nm / NiCr 5nm / AZO 12nm / SiN x 22nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0144] Example 1

[0145] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked ZnSnO. x 25nm / AZO 15nm / Ag 10nm / AZO 10nm / ZnSnO x 48nm / AZO 16nm / Ag 11nm / AZO 10nm / SiN x 62nm / W 15nm / SiN x 10nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0146] Example 2

[0147] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked ZnSnO. x 25nm / AZO 15nm / Ag 10nm / AZO 10nm / ZnSnO x 48nm / AZO 16nm / Ag 11nm / AZO 10nm / SiN x 62nm / NiCr 15nm / SiN x 10nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0148] Example 3

[0149] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked ZnSnO. x 25nm / AZO 17nm / Ag 10nm / AZO 10nm / ZnSnO x 46nm / AZO 16nm / Ag 11nm / AZO 10nm / SiN x 65nm / Ti 19nm / SiN x 12nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0150] Example 4

[0151] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked layers of SiN... x 30nm / AZO 15nm / Ag10nm / AZO 10nm / SiN x 52nm / AZO 18nm / Ag 11nm / AZO 10nm / SiN x 15nm / W 5nm / SiN x 55nm / W7nm / SiN x 10nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0152] Example 5

[0153] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked layers of SiN... x 30nm / AZO 15nm / Ag10nm / AZO 10nm / SiN x 54nm / AZO 18nm / Ag 11nm / AZO 10nm / SiN x 15nm / NiCr 8nm / SiN x 52nm / NiCr 10.5nm / SiN x 13nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0154] Example 6

[0155] This embodiment provides a laminated glass, including an outer glass substrate and an inner glass substrate. The outer glass substrate is made of clear glass with a geometric thickness of 2.1 mm, and the inner glass substrate is made of gray glass with a geometric thickness of 2.1 mm and a transmittance of 25%~30%. An infrared-reflective low-emissivity film is deposited on the inner surface of the outer glass substrate using magnetron sputtering. The film comprises, from the direction near the inner surface of the outer glass substrate to the direction away from the inner surface of the outer glass substrate, sequentially stacked layers of SiN... x 30nm / AZO 15nm / Ag10nm / AZO 10nm / SiN x 54nm / AZO 18nm / Ag 11nm / AZO 10nm / SiN x 15nm / Ti 8nm / SiN x 52nm / Ti 14nm / SiN x 13nm. After coating, both the outer and inner glass substrates undergo heat treatment at 550℃~650℃. The outer and inner glass substrates are then bonded together using a transparent PVB adhesive layer with a transmittance of ≥90%.

[0156] The characterization data of the laminated glass in the above embodiments and comparative examples are shown in Tables 1 and 2 below.

[0157] Table 1 Performance data of laminated coated glass in Comparative Examples 1-4 and Example 1

[0158]

[0159] As can be seen from Comparative Examples 1 to 4 in Table 1, Comparative Example 1 is a traditional double-silver heat-reflective coated laminated glass without a metal absorption layer. It usually requires a PVB adhesive layer with low transmittance to bond the laminated glass, so that the laminated glass has low visible light transmittance, low visible light reflectance (<15%) and low total solar energy transmittance (≤20%). However, the price of low-transmittance PVB adhesive layer is usually more expensive than transparent PVB, which increases the cost.

[0160] In Comparative Example 2, the laminated glass used a combination of two pieces of clear glass and transparent PVB. Although the film layer in Comparative Example 2 used NiCr (nickel-chromium alloy) as a metal absorption layer and placed one of the NiCr layers between the two Ag layers, it could reduce the visible light transmittance of the coated glass and the visible light transmittance of the laminated glass to a certain extent. However, its visible light reflectance Rl was too high, reaching 23.50%.

[0161] Comparative Example 3, using the same glass configuration as Comparative Example 2, further increases the total geometric thickness of the metal absorbing layer. Although this can further reduce the visible light transmittance and total solar energy transmittance of the laminated glass to some extent, it is evident that the visible light reflectance Rl also increases significantly with the increase in the geometric thickness of the metal absorbing layer. This causes a certain degree of light pollution, which is detrimental to the appearance of the laminated coated glass. At the same time, the color component b value of the reflected color of the laminated glass in the Lab color space is less than -15, which will cause the overall reflected color of the glass to be bluish.

[0162] In Comparative Example 4, the laminated glass used a combination of clear glass, gray glass, and transparent PVB. While using a metal absorbing layer in the film layer, the inner glass substrate of the laminated glass was replaced with low-transmittance gray glass, which also made the visible light transmittance and total solar energy transmittance of the laminated glass similar to those of the traditional laminated coated glass using gray PVB in Comparative Example 1. However, the visible light reflectance was still relatively high. At the same time, the color component a value of the reflected color of the laminated glass in the Lab color space was less than -5, which caused the overall reflected color of the glass to be greenish.

[0163] In Example 1, using the same glass configuration as Comparative Example 4, by placing the metal absorbing layer on the side away from the first glass substrate from all infrared reflective metal layers, and without using low-transmittance gray PVB, its visible light reflectance Rl is significantly reduced compared to Comparative Example 4, and its visible light transmittance is also reduced compared to Comparative Examples 1 to 4. Furthermore, other properties of its laminated coated glass are essentially close to those of Comparative Example 1, achieving superior cost control while satisfying requirements for low visible light transmittance, visible light reflectance, total solar energy transmittance, and aesthetically pleasing color properties.

[0164] Table 2 Performance data of laminated coated glasses in Examples 1-6

[0165]

[0166] Table 2 shows that Examples 1-6 all used the same glass configuration as Comparative Example 4. Overall, the film systems in Examples 1-6 showed better performance in all parameters compared to Comparative Example 4. Even without using low-transmittance gray PVB, the visible light reflectance Rl of Examples 1-6 was significantly lower than that of Comparative Example 4, and the visible light transmittance was also lower. Furthermore, other parameters of their laminated coated glass were essentially close to those of Comparative Example 1, achieving superior cost control while meeting requirements for lower visible light transmittance, visible light reflectance, total solar energy transmittance, and aesthetically pleasing color.

[0167] Among them, Examples 1 to 3 are schemes that use a single metal absorbing layer. They have fewer film layers and the process complexity during coating is relatively lower. The reflected color of the laminated glass in Examples 1 to 3 is more neutral than that in Comparative Examples 3 and 4. It can be seen that the single metal absorbing layer scheme has lower visible light reflectance and visible light transmittance than the schemes in Comparative Examples 3 and 4 that use double metal absorbing layers, and it is also more neutral in color performance.

[0168] Table 2 shows examples 4-6, which employ a two-layer metal absorbing layer coating technique. Compared to Comparative Examples 3 and 4, both metal absorbing layers in Examples 4-6 are located on the side of all infrared reflective metal layers furthest from the first glass substrate. This film design results in lower visible light reflectance and visible light transmittance compared to the double-layer metal absorbing layer schemes used in Comparative Examples 3 and 4. Furthermore, the two-layer metal absorbing layer coating techniques in Examples 4-6 exhibit a greater bias towards neutral colors in the Lab color space compared to Examples 1-3, thus demonstrating better color performance.

[0169] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0170] The above-described embodiments are merely illustrative of several implementation methods of the present invention, facilitating a detailed understanding of the technical solutions of the present invention, but should not be construed as limiting the scope of protection of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. It should be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided by the present invention through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this invention patent should be determined by the content of the appended claims, and the specification and drawings can be used to interpret the content of the claims.

Claims

1. A low-emissivity coated glass, characterized in that, The device includes a first glass substrate and a coating layer disposed on at least one surface of the first glass substrate. The coating layer includes at least two infrared reflective metal layers and at least one metal absorbing layer stacked on top of each other. The metal absorbing layer is disposed on the side of all infrared reflective metal layers away from the first glass substrate. Wherein, the geometric thickness of the metal absorption layer is ≥7nm; A second intermediate dielectric layer is provided between the metal absorbing layer and the infrared reflective metal layer.

2. The low-emissivity coated glass according to claim 1, characterized in that, The coating layer includes an inner dielectric layer, a first infrared reflective metal layer, a first intermediate dielectric layer, a second infrared reflective metal layer, a second intermediate dielectric layer, a metal absorption layer, and an outer dielectric layer stacked sequentially, wherein the inner dielectric layer is closer to the first glass substrate than the outer dielectric layer.

3. The low-emissivity coated glass according to claim 1 or 2, characterized in that, The metal absorption layer satisfies one or more of the following conditions: (1) The material of the metal absorption layer includes one or more alloys of W, Ni, Cr, Ti, Nb, Mo, Si and Zr; (2) The total geometric thickness of the metal absorption layer disposed on the side of all infrared reflective metal layers away from the first glass substrate is ≥7nm, and the total geometric thickness of the metal absorption layer is ≤50nm.

4. The low-emissivity coated glass according to claim 3, characterized in that, The material of the metal absorption layer includes one of W, Ti, and NiCr.

5. The low-emissivity coated glass according to claim 3, characterized in that, The metal absorption layer includes a first metal layer close to the first glass substrate and a second metal layer further away from the first glass substrate than the first metal layer, wherein the first metal layer and the second metal layer satisfy one or more of the following conditions: (1) The geometric thickness of the first metal layer is ≥2nm; (2) The geometric thickness of the second metal layer is ≥5nm; (3) A third intermediate dielectric layer is provided between the first metal layer and the second metal layer.

6. The low-emissivity coated glass according to claim 5, characterized in that, The geometric thickness of the third intermediate dielectric layer is 20nm~80nm.

7. The low-emissivity coated glass according to claim 5, characterized in that, The material of the third intermediate dielectric layer includes an oxide of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

8. The low-emissivity coated glass according to claim 1 or 2, characterized in that, The infrared reflective metal layer satisfies one or more of the following conditions: (1) The material of each infrared reflective metal layer independently includes any one or more alloys of Ag, Au, Cu, Al, Pt, Pd, Mo and In; (2) The geometric thickness of each infrared reflective metal layer is independently 5nm~20nm.

9. The low-emissivity coated glass according to claim 8, characterized in that, The material of each of the infrared reflective metal layers includes Ag.

10. The low-emissivity coated glass according to claim 2, characterized in that, The inner dielectric layer satisfies one or more of the following conditions: (1) The material of the inner dielectric layer includes one or more of the oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more of the nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta. (2) The geometric thickness of the inner dielectric layer is 15nm~50nm.

11. The low-emissivity coated glass according to claim 2, characterized in that, The first intermediate dielectric layer satisfies one or more of the following conditions: (1) The geometric thickness of the first intermediate dielectric layer is 40 nm to 100 nm; (2) The material of the first intermediate dielectric layer includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta.

12. The low-emissivity coated glass according to claim 2, characterized in that, The second intermediate dielectric layer satisfies one or more of the following conditions: (1) The material of the second intermediate dielectric layer includes one or more oxides of at least one element selected from Zn, Si, Sn, Ti, Nb, Zr, Hf, Mg, Ni, In, Al, Ga, W and Bi, or one or more nitrides and oxynitrides of at least one element selected from Si, Al, Zr, Ti, Y, Hf, Nb and Ta. (2) The geometric thickness of the second intermediate dielectric layer is 10nm~100nm.

13. The low-emissivity coated glass according to claim 12, characterized in that, The material of the second intermediate dielectric layer includes SiN x .

14. The low-emissivity coated glass according to claim 2, characterized in that, The outer dielectric layer satisfies one or more of the following conditions: (1) The geometric thickness of the outer dielectric layer is ≥5nm; (2) The material of the outer dielectric layer includes one or more of the nitrides and oxides of at least one of the elements selected from Si, Al, Zr, Ti and B.

15. The low-emissivity coated glass according to claim 14, characterized in that, The material of the outer dielectric layer includes SiN. x .

16. The low-emissivity coated glass according to claim 2, characterized in that, The coating layer further includes a first barrier layer and / or a second barrier layer. The first barrier layer is disposed between the first infrared reflective metal layer and the first intermediate dielectric layer. The geometric thickness of the first barrier layer is 0.5 nm to 10 nm. The material of the first barrier layer includes one or more of the metals, alloys, oxides and nitrides of at least one element selected from Ni, Cr, Ti, Zn, Nb, Hf, Zr and Al. The second barrier layer is disposed between the second infrared reflective metal layer and the second intermediate dielectric layer. The geometric thickness of the second barrier layer is 0.5 nm to 10 nm. The material of the second barrier layer includes one or more of the metals, alloys, oxides and nitrides of at least one element, such as Ni, Cr, Ti, Zn, Nb, Hf, Zr and Al.

17. A laminated glass, characterized in that, The laminated glass includes the low-emissivity coated glass according to any one of claims 1 to 16, an adhesive layer, and a second glass substrate, wherein the adhesive layer is disposed between the coated layer and the second glass substrate and is located on the side surface of the coated layer away from the first glass substrate.

18. The laminated glass according to claim 17, characterized in that, The visible light transmittance of the first glass substrate is ≥70%, the visible light transmittance of the second glass substrate is ≤50%, and the visible light transmittance of the adhesive layer is ≥70%.

19. The laminated glass according to claim 17, characterized in that, The visible light transmittance of the laminated glass is ≤10%.

20. The laminated glass according to claim 17, characterized in that, The visible light reflectance of the laminated glass is ≤20%.

21. The laminated glass according to claim 17, characterized in that, The total solar transmittance of the laminated glass is ≤25%.

22. The laminated glass according to claim 17, characterized in that, The reflected color of the laminated glass surface has a color component L value of 0~60, a value of -5~0, and a value of -15~0 in the Lab color space.

23. A vehicle, characterized in that, Includes the laminated glass as described in any one of claims 17 to 22.

Citation Information

Patent Citations

  • Low emissivity coating with low solar heat gain coefficient, enhanced chemical and mechanical properties and method of making the same