Ink, thin film, and method of preparation, optoelectronic device, display device
By using polymer materials with different molecular weights in OLED and QLED devices, the uniformity of ink film formation was adjusted, solving the problem of uneven functional layer film formation and improving device performance and the uniformity of large-size display panels.
Patent Information
- Application Number
- CN202211724736.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-12-30
AI Technical Summary
In the existing technology, OLED and QLED devices prepared by solution method have the problem of uneven functional layer film formation, which leads to reduced device performance. In particular, it is difficult to achieve high uniformity of the dried film in large-size and high-resolution display panels.
The ink uses a mixture of polymer materials. The first polymer material has a high weight-average molecular weight of 50,000 g/mol to 150,000 g/mol, while the second polymer material has a weight-average molecular weight of 10,000 g/mol to 50,000 g/mol. By adjusting the migration speed of the polymer and its interaction with the substrate, convex and concave film morphologies are formed, thereby improving the uniformity of film formation.
This improved the uniformity of the functional layer film formation, ensured the adjustment of charge transport characteristics and film morphology, and enhanced device performance.
Smart Images

Figure CN117683404B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of display technology, and in particular to an ink, a thin film and its preparation method, an optoelectronic device, and a display apparatus. Background Technology
[0002] In the fabrication processes of organic light-emitting diodes (OLEDs) and quantum dot light-emitting diodes (QLEDs), solvent-based methods such as inkjet printing can be used to prepare light-emitting functional layers, including electron injection layers, electron transport layers, hole injection layers, hole transport layers, and light-emitting layers. This involves depositing functional material ink into pixel pits on a substrate and then drying the ink to form the corresponding light-emitting functional layers. However, devices fabricated using solution methods suffer from uneven functional layer formation, leading to reduced device performance.
[0003] There are two main reasons for uneven film formation during drying: (1) the coffee ring phenomenon caused by outward capillary flow, resulting in a thinner film in the middle and a thicker film at the edges; and (2) inward Maragonian flow, resulting in a film that is thicker in the middle and thinner at the edges. Therefore, the idea of controlling the uniformity of film formation is to balance the two forces or weaken one of them. Subramanian et al. found that when the substrate temperature dropped to 17°C, the evaporation rates at the edge and center of the droplet were similar, reducing the outward capillary flow of the droplet and thus weakening the coffee ring effect. Moon et al. used ethylene glycol, which has a high boiling point and low surface tension, as a solvent. Because ethylene glycol has a slow evaporation rate, as the solvent evaporates, the concentration of ethylene glycol in the edge region gradually becomes higher than that in the center region. A surface tension difference is generated between the droplet edge and the center, causing inward Maragonian flow.
[0004] Currently, methods to improve film uniformity in production include optimizing the ratio of high- and low-boiling-point solvents in the ink system and adjusting the evaporation rate of the solvent by optimizing vacuum drying process parameters. However, with the increase in display panel size and resolution, relying solely on traditional adjustment methods is insufficient to achieve high uniformity in the dried film. In particular, methods involving selecting or changing the type of solvent encounter bottlenecks, and changing the solvent can also affect the processability of inkjet printing, requiring consideration of whether the new solvent will damage the underlying film layer. Summary of the Invention
[0005] Therefore, it is necessary to provide an ink, a thin film and its preparation method, an optoelectronic device, and a display device to improve the uniformity of ink film formation.
[0006] An ink, characterized in that it comprises a solvent and a solute, wherein the solute comprises a first polymer material and a second polymer material, wherein the weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0007] In one embodiment, the weight-average molecular weight of the first polymer material is 100,000 g / mol to 200,000 g / mol, and the weight-average molecular weight of the second polymer material is 10,000 g / mol to 50,000 g / mol.
[0008] In one embodiment, the first polymer material accounts for 50%-90% of the mass fraction of the solute, and the second polymer material accounts for 10%-50% of the mass fraction of the solute.
[0009] In one embodiment, the first polymer material and the second polymer material are each independently selected from poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine).
[0010] In one embodiment, the first polymer material and the second polymer material are poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid.
[0011] In one embodiment, the first polymer material and the second polymer material are each independently selected from at least one of poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenyleneethylene, poly(2-(4-(3',7'-dimethyloctyloxyphenyl)-1,4-phenyleneethylene) and poly(9,9-dioctyl-9H-fluorene-2,7-diyl).
[0012] In one embodiment, the first polymer material and the second polymer material are the same polymer.
[0013] A method for preparing a thin film includes the following steps:
[0014] The ink described in any of the above embodiments is applied to a substrate and dried to form a film.
[0015] A thin film comprising a mixture of a first polymer material and a second polymer material, wherein the weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0016] An optoelectronic device includes a first electrode layer, a functional layer, and a second electrode layer stacked together. The material of the functional layer includes a mixture of a first polymer material and a second polymer material. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0017] In one embodiment, the functional layer includes a light-emitting layer, the material of which is selected from at least one of poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene, poly(2-(4-(3',7'-dimethyloctyloxyphenyl)-1,4-phenylenevinylene), and poly(9,9-dioctyl-9H-fluorene-2,7-diyl);
[0018] The functional layer further includes a hole injection layer and / or a hole transport layer. The hole injection layer is made of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid, and the hole transport layer is made of at least one selected from poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine).
[0019] In one embodiment, the materials of the first electrode layer and the second electrode layer are independently selected from one or more of metals, carbon materials, and metal oxides. The metals include one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg. The carbon materials include one or more of graphite, carbon nanotubes, graphene, and carbon fibers. The metal oxides include doped or undoped metal oxides, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or composite electrodes consisting of metal sandwiched between doped or undoped transparent metal oxides. The composite electrodes include one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2.
[0020] A display device comprising the optoelectronic device described in any of the above embodiments.
[0021] Compared with traditional solutions, the above-mentioned inks have the following beneficial effects:
[0022] The study found that during solvent evaporation, polymers with higher molecular weight migrate more slowly and have a stronger interaction force with the substrate, making them more likely to form convex film morphologies under certain drying conditions. In contrast, polymers with lower molecular weight exhibit the opposite trend and are more likely to form concave film morphologies.
[0023] The aforementioned ink utilizes the wide molecular weight distribution of polymers, employing a combination of high- and low-molecular-weight polymers as the solute to regulate film uniformity. More specifically, a first polymer material and a second polymer material are combined. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The higher weight-average molecular weight of the first polymer material ensures the film formation and charge transport characteristics of the functional layer, and it easily forms a convex film morphology when dried alone. The lower weight-average molecular weight serves as an auxiliary component, and it easily forms a concave film morphology when dried alone, acting as a film morphology modifier. The combination of the two improves the uniformity of ink film formation. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of film formation using polymers with high molecular weight.
[0025] Figure 2 A schematic diagram of film formation using polymers with low molecular weight;
[0026] Figure 3 In the middle (1) and (2), the film thickness detection diagrams of two TFB samples with weight average molecular weight of 100,000 g / mol to 200,000 g / mol are respectively.
[0027] Figure 4 In the middle (1) and (2), the film thickness detection diagrams are respectively of two TFB samples with weight average molecular weight of 10,000 g / mol and 50,000 g / mol;
[0028] Figure 5 This is a schematic diagram of the structure of an optoelectronic device according to an embodiment;
[0029] Explanation of reference numerals in the attached figures:
[0030] 100. Optoelectronic device; 110. First electrode layer; 130. Functional layer; 131. Light-emitting material layer; 132. Hole transport layer; 133. Hole injection layer; 150. Second electrode layer. Detailed Implementation
[0031] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Preferred embodiments of the invention are shown in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the invention.
[0032] It should be noted that when a component is said to be "set on" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0034] An embodiment of the ink of the present invention includes a solvent and a solute. The solute includes a first polymer material and a second polymer material, wherein the weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0035] Studies have found that during solvent evaporation, polymers with higher molecular weights migrate more slowly and have stronger interactions with the substrate, making them more likely to form convex film morphologies under certain drying conditions. Figure 1 The film formation 10 of this polymer is schematically shown. Polymers with lower molecular weights, on the other hand, tend to form concave film morphologies. Figure 2 The film formation of the polymer is schematically shown 20.
[0036] The aforementioned ink utilizes the wide molecular weight distribution of polymers used in hole transport or hole injection materials. The solutes are a combination of high- and low-molecular-weight polymers to regulate film uniformity. More specifically, a first polymer material and a second polymer material are used in combination. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The higher weight-average molecular weight of the first polymer material ensures the film formation and charge transport characteristics of the functional layer, and it easily forms a convex film morphology when dried alone. The lower weight-average molecular weight serves as an auxiliary component, and it easily forms a concave film morphology when dried alone, acting as a film morphology modifier. The combination of the two improves the uniformity of the ink film formation.
[0037] In one example, the weight-average molecular weight of the first polymer material is 100,000 g / mol to 200,000 g / mol, and the weight-average molecular weight of the second polymer material is 10,000 g / mol to 50,000 g / mol.
[0038] In the above example, a first polymer material with a weight-average molecular weight of 100,000 g / mol to 200,000 g / mol is used as the main component to ensure the film formation and charge transport characteristics of the functional layer; a second polymer material with a weight-average molecular weight of 10,000 g / mol to 50,000 g / mol is used as an auxiliary component to act as a film morphology modifier, thereby improving the uniformity of ink film formation.
[0039] In one example, the first polymer material accounts for 50%-90% of the mass fraction of the solute, and the second polymer material accounts for 10%-50% of the mass fraction of the solute.
[0040] In one example, both the first polymer material and the second polymer material are either hole transport materials, hole injection materials, or luminescent materials. Examples of hole transport materials include, but are not limited to: poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine) (TFB, CAS No. 223569-31-1), polyvinylcarbazole (PVK, CAS No. 25067-59-8), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) (Poly-TPD, CAS No. 472960-35-3), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine). Examples of hole injection materials include, but are not limited to: poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid (PEDOT:PSS, CAS No. 155090-83-8). As a luminescent material, it can be, for example, but not limited to: poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene (MEH-PPV, CAS No. 138184-36-8), poly(2-(4-(3',7'-dimethyloctyloxyphenyl)-1,4-phenylenevinylene)(P-PPV), poly(9,9-dioctyl-9H-fluorene-2,7-diyl)(PFO, CAS No. 195456-48-5).
[0041] like Figure 3 As shown, (1) and (2) are film thickness detection diagrams of two TFB samples with weight average molecular weight of 100,000 g / mol to 200,000 g / mol, respectively. It can be seen that TFB samples with this molecular weight form a convex film morphology when dried alone.
[0042] like Figure 4 As shown, (1) and (2) are film thickness detection diagrams of two TFB samples with weight average molecular weight of 10,000 g / mol to 50,000 g / mol, respectively. It can be seen that TFB samples with this molecular weight form a concave film morphology when dried alone.
[0043] In one example, the first polymer material and the second polymer material are the same polymer.
[0044] Optionally, the solvent may be, for example, but not limited to, alkyl benzoate, aralkyl benzoate, alkyl ether, polycyclic aromatic hydrocarbon, etc.
[0045] Furthermore, the present invention also provides a method for preparing a thin film, comprising the following steps:
[0046] The ink described above is applied to the substrate and dried to form a film.
[0047] The thin film can be a light-emitting material thin film, a hole transport thin film, or a hole injection thin film, etc.
[0048] The ink coating method can be, for example, spin coating, inkjet printing, etc.
[0049] Furthermore, the present invention also provides a thin film whose material comprises a mixture of a first polymer material and a second polymer material, wherein the weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0050] The thin film can be a light-emitting material thin film, a hole transport thin film, or a hole injection thin film, etc.
[0051] The aforementioned film comprises a mixture of a first polymer material and a second polymer material. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The first polymer material, with its higher weight-average molecular weight, ensures the film formation and charge transport characteristics of the functional layer and easily forms a convex film morphology when dried alone. The second polymer material, with its lower weight-average molecular weight, serves as an auxiliary component and easily forms a concave film morphology when dried alone, thus acting as a film morphology modifier. The combination of the two can improve the uniformity of ink film formation.
[0052] Furthermore, such as Figure 5 As shown, the present invention also provides an optoelectronic device 100, comprising a first electrode layer 110, a functional layer 130, and a second electrode layer 150 stacked together. The material of the functional layer 130 comprises a mixture of a first polymer material and a second polymer material, wherein the weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material.
[0053] The functional layer 130 includes a light-emitting material layer 131, and may further include a hole transport layer 132 and / or a hole injection layer 133.
[0054] When the functional layer 130 further includes a hole transport layer 132 and a hole injection layer 133, the hole injection layer 133 is disposed between the hole transport layer 132 and the second electrode layer 150.
[0055] In one example, at least one of the hole transport layer 132 and the hole injection layer 133 comprises a mixture of a first polymer material and a second polymer material.
[0056] In one example, the hole transport layer 132 is made of a mixture of a first polymer material and a second polymer material. The first and second polymer materials may be, for example, but not limited to, TFB, PVK, Poly-TPD, etc.
[0057] In one example, the material of the hole injection layer 133 comprises a mixture of a first polymer material and a second polymer material. The first polymer material and the second polymer material may be, for example, but not limited to, PEDOT:PSS.
[0058] It is understood that one or more layers of functional layer 130 can be obtained by coating with the above-mentioned ink and then drying.
[0059] In one example, the luminescent material layer 120 comprises a mixture of a first polymer material and a second polymer material. The first polymer material and the second polymer material may be, for example, but not limited to, MEH-PPV, P-PPV, PFO, etc.
[0060] Furthermore, the first and second polymer materials in the luminescent material layer 120 are not limited to luminescent materials. For example, the luminescent material layer 120 may also be composed of a first polymer material, a second polymer material, and a phosphorescent material doped in the aforementioned polymer materials. Phosphorescent materials may be, for example, but not limited to, Ir(piq)3, Ir(mppy)3, Firpic, etc.
[0061] In one example, the luminescent material layer 120 includes a first polymer material, a second polymer material, and a phosphorescent material Ir(piq)3. Both the first and second polymer materials are PVK, and the mass ratio of the polymer material to the phosphorescent material is 100:2.
[0062] In one example, the luminescent material layer 120 includes a first polymer material, a second polymer material, and a phosphorescent material Ir(mppy)3. Both the first and second polymer materials are PVK, and the mass ratio of the polymer material to the phosphorescent material is 100:4.
[0063] In one example, the luminescent material layer 120 includes a first polymer material, a second polymer material, and a phosphorescent material Firpic. Both the first and second polymer materials are PVK, and the mass ratio of the polymer material to the phosphorescent material is 100:10.
[0064] In addition, the light-emitting material layer 120 can also be a conventional light-emitting material, such as a quantum dot light-emitting layer or an organic light-emitting layer.
[0065] In one example, the material of the quantum dot emitting layer includes at least one of single-structure quantum dots and core-shell structure quantum dots. The material of the single-structure quantum dots is selected from at least one of group II-VI compounds, group IV-VI compounds, group III-V compounds, and group I-III-VI compounds. Specifically, the group II-VI compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe. At least one of HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, and HgZnSTe, wherein the IV-VI compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnS At least one of the following: eS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe; and a III-V compound selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, and AlPA. The quantum dots are selected from at least one of the following: s, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, or InAlPSb. The I-III-VI group compounds are selected from at least one of CuInS2, CuInSe2, and AgInS2. The core of the core-shell quantum dot includes any one of the above-mentioned single-structure quantum dots, and the shell material of the core-shell quantum dot includes at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS, and the above-mentioned single-structure quantum dots.
[0066] In one example, the material of the organic light-emitting layer includes at least one of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine-C2,N)iridium(III), 4,4',4”-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine-C2,N)iridium, diaromatic anthracene derivatives, stilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials and DBP fluorescent materials, polyacetylene and its derivatives, poly(p-phenylene) and its derivatives, polythiophene and its derivatives, and polyfluorene and its derivatives.
[0067] In one example, the materials of the first electrode layer 110 and the second electrode layer 150 are independently selected from one or more of metals, carbon materials, and metal oxides. Metals include one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg. Carbon materials include one or more of graphite, carbon nanotubes, graphene, and carbon fibers. Metal oxides include doped or undoped metal oxides, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or composite electrodes consisting of metal sandwiched between doped or undoped transparent metal oxides. These composite electrodes include one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2.
[0068] Furthermore, the present invention also provides a display device including the optoelectronic device of any of the above examples.
[0069] Display devices can be, but are not limited to, computers, tablets, mobile phones, televisions, smartwatches, AR / VR devices, etc.
[0070] The present invention will be further illustrated by specific embodiments provided below.
[0071] Example 1
[0072] This embodiment provides a method for fabricating an optoelectronic device, including the following steps:
[0073] Step 1: Print hole injection material PEDOT:PSS on a substrate with an anode layer, vacuum dry it to form a film, and then heat it at 200°C for 30 minutes to form a hole injection layer.
[0074] Step 2: Print hole transport material onto the hole injection layer, vacuum dry to form a film, and then heat at 200℃ for 30 minutes to form the hole transport layer. The hole transport material is composed of TFB with different molecular weights, of which 80% has a weight-average molecular weight of 100,000 g / mol to 200,000 g / mol, and 20% has a weight-average molecular weight of 10,000 g / mol to 50,000 g / mol.
[0075] Step 3: Print the luminescent material onto the hole transport layer, vacuum dry it to form a film, and then heat it at 140°C for 15 minutes to form a luminescent material layer.
[0076] Step 4: Co-deposit TSPO1:Liq on the above-mentioned luminescent material layer at a weight ratio of 5:5, with both deposition rates being [missing information]. Vacuum degree is 2×10 -4 Pa forms an electron transport layer with a thickness of 30 nm.
[0077] Step 5: Deposit a Mg:Ag alloy onto the electron transport layer, with a Mg:Ag weight ratio of 1:9, and control the deposition rates of both alloys to be as follows: and Vacuum degree controlled at 2×10 -4 Pa forms a semi-transparent cathode with a thickness of 15 nm.
[0078] Step 6: Deposit an IZO thin film on the semi-transparent cathode using a low-temperature sputtering process. The sputtering power is controlled at 5 kW and the process pressure is controlled at 1 Pa to form a light extraction layer with a thickness of 70 nm.
[0079] Step 7: Prepare stacked SiN layers on the above-mentioned light extraction layer. x / Organic thin film / SiN x SiN x The organic thin film was prepared by CVD process with a thickness of 1 μm, and the organic thin film was prepared by IJP process with a thickness of 10 μm.
[0080] Example 2
[0081] This embodiment provides a method for fabricating an optoelectronic device, including the following steps:
[0082] Step 1: Print hole injection material PEDOT:PSS on a substrate with an anode layer, vacuum dry it to form a film, and then heat it at 200°C for 30 minutes to form a hole injection layer.
[0083] Step 2: Print hole transport material onto the hole injection layer, vacuum dry to form a film, and then heat at 200℃ for 30 minutes to form the hole transport layer. The hole transport material is composed of Poly-TPDs with different molecular weights, of which 80% have a weight-average molecular weight of 100,000 g / mol to 200,000 g / mol, and 20% have a weight-average molecular weight of 10,000 g / mol to 50,000 g / mol.
[0084] Step 3: Print the luminescent material onto the hole transport layer, vacuum dry it to form a film, and then heat it at 140°C for 15 minutes to form a luminescent material layer.
[0085] Step 4: Co-deposit TSPO1:Liq on the above-mentioned luminescent material layer at a weight ratio of 5:5, with both deposition rates being [missing information]. Vacuum degree is 2×10 -4 Pa forms an electron transport layer with a thickness of 30 nm.
[0086] Step 5: Deposit a Mg:Ag alloy onto the electron transport layer, with a Mg:Ag weight ratio of 1:9, and control the deposition rates of both alloys to be as follows: and Vacuum degree controlled at 2×10 -4 Pa forms a semi-transparent cathode with a thickness of 15 nm.
[0087] Step 6: Deposit an IZO thin film on the semi-transparent cathode using a low-temperature sputtering process. The sputtering power is controlled at 5 kW and the process pressure is controlled at 1 Pa to form a light extraction layer with a thickness of 70 nm.
[0088] Step 7: Prepare stacked SiN layers on the above-mentioned light extraction layer. x / Organic thin film / SiN x SiN x The organic thin film was prepared by CVD process with a thickness of 1 μm, and the organic thin film was prepared by IJP process with a thickness of 10 μm.
[0089] Example 3
[0090] This embodiment provides a method for fabricating an optoelectronic device, including the following steps:
[0091] Step 1: Print hole injection material PEDOT:PSS on a substrate with an anode layer, vacuum dry to form a film, and then heat at 200℃ for 30 min to form a hole injection layer. The hole injection material is composed of PEDOT:PSS with different molecular weights, of which 75% have a weight-average molecular weight of 100,000 g / mol to 200,000 g / mol, and 25% have a weight-average molecular weight of 10,000 g / mol to 50,000 g / mol.
[0092] Step 2: Print hole transport material TFB onto the hole injection layer, vacuum dry it to form a film, and then heat it at 200°C for 30 minutes to form a hole transport layer.
[0093] Step 3: Print the luminescent material onto the hole transport layer, vacuum dry it to form a film, and then heat it at 140°C for 15 minutes to form a luminescent material layer.
[0094] Step 4: Co-deposit TSPO1:Liq on the above-mentioned luminescent material layer at a weight ratio of 5:5, with both deposition rates being [missing information]. Vacuum degree is 2×10 -4 Pa forms an electron transport layer with a thickness of 30 nm.
[0095] Step 5: Deposit a Mg:Ag alloy onto the electron transport layer, with a Mg:Ag weight ratio of 1:9, and control the deposition rates of both alloys to be as follows: and Vacuum degree controlled at 2×10 -4 Pa forms a semi-transparent cathode with a thickness of 15 nm.
[0096] Step 6: Deposit an IZO thin film on the semi-transparent cathode using a low-temperature sputtering process. The sputtering power is controlled at 5 kW and the process pressure is controlled at 1 Pa to form a light extraction layer with a thickness of 70 nm.
[0097] Step 7: Prepare stacked SiN layers on the above-mentioned light extraction layer. x / Organic thin film / SiN x SiN x The organic thin film was prepared by CVD process with a thickness of 1 μm, and the organic thin film was prepared by IJP process with a thickness of 10 μm.
[0098] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0099] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims, and the specification can be used to interpret the content of the claims.
Claims
1. An ink, characterized in that, The mixture includes a solvent and a solute, wherein the solute is a first polymer material and a second polymer material. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The weight-average molecular weight of the first polymer material is 100,000 g / mol to 200,000 g / mol, and the weight-average molecular weight of the second polymer material is 10,000 g / mol to 50,000 g / mol. The first polymer material accounts for 50% to 90% of the mass fraction of the solute, and the second polymer material accounts for 10% to 50% of the mass fraction of the solute. The second polymer material is used to adjust the morphology of the film formed by the ink. The first polymer material and the second polymer material are each independently selected from at least one of poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine); or, the first polymer material and the second polymer material are poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid; or, the first polymer material and the second polymer material are each independently selected from at least one of poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenyleneethylene], poly(2-(4-(3',7'-dimethyloctyloxy)phenyl)-1,4-phenyleneethylene), and poly(9,9-dioctyl-9H-fluorene-2,7-diyl).
2. The ink as described in claim 1, characterized in that, The solvent is at least one of alkyl benzoate, aralkyl benzoate, alkyl ether, and polycyclic aromatic hydrocarbon.
3. The ink as described in claim 1 or 2, characterized in that, The first polymer material and the second polymer material are the same polymer.
4. A method for preparing a thin film, characterized in that, Includes the following steps: The ink used in any one of claims 1 to 3 is applied to the substrate and dried to form a film.
5. A thin film, characterized in that, The film is made of a mixture of a first polymer material and a second polymer material. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The weight-average molecular weight of the first polymer material is 100,000 g / mol to 200,000 g / mol, and the weight-average molecular weight of the second polymer material is 10,000 g / mol to 50,000 g / mol. The first polymer material accounts for 50% to 90% of the mass fraction of the solute, and the second polymer material accounts for 10% to 50% of the mass fraction of the solute. The solute is a mixture of the first polymer material and the second polymer material, and the second polymer material is used to adjust the morphology of the film. The first polymer material and the second polymer material are each independently selected from at least one of poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine); or, the first polymer material and the second polymer material are poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid; or, the first polymer material and the second polymer material are each independently selected from at least one of poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenyleneethylene], poly(2-(4-(3',7'-dimethyloctyloxy)phenyl)-1,4-phenyleneethylene), and poly(9,9-dioctyl-9H-fluorene-2,7-diyl).
6. An optoelectronic device, characterized in that, The device comprises a first electrode layer, a functional layer, and a second electrode layer stacked together. The functional layer is made of a mixture of a first polymer material and a second polymer material. The weight-average molecular weight of the first polymer material is 50,000 g / mol to 150,000 g / mol higher than that of the second polymer material. The weight-average molecular weight of the first polymer material is 100,000 g / mol to 200,000 g / mol, and the weight-average molecular weight of the second polymer material is 10,000 g / mol to 50,000 g / mol. The first polymer material accounts for 50% to 90% of the mass fraction of the solute, and the second polymer material accounts for 10% to 50% of the mass fraction of the solute. The solute is a mixture of the first and second polymer materials, and the second polymer material is used to adjust the morphology of the functional layer. The functional layer includes a light-emitting layer, the material of which is selected from at least one of poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene], poly(2-(4-(3',7'-dimethyloctyloxy)phenyl)-1,4-phenylenevinylene) and poly(9,9-dioctyl-9H-fluorene-2,7-diyl); The functional layer further includes a hole injection layer and / or a hole transport layer. The hole injection layer is made of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid, and the hole transport layer is made of at least one selected from poly(9,9-dioctylfluorene-CO-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), and poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine).
7. The optoelectronic device as described in claim 6, characterized in that, The materials of the first electrode layer and the second electrode layer are independently selected from one or more of metals, carbon materials, and metal oxides. The metals include one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg. The carbon materials include one or more of graphite, carbon nanotubes, graphene, and carbon fibers. The metal oxides include doped or undoped metal oxides, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or composite electrodes consisting of metal sandwiched between doped or undoped transparent metal oxides. The composite electrodes include one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2.
8. A display device, characterized in that, Including the optoelectronic device as described in claim 6 or 7.
Citation Information
Patent Citations
Ink for ink-jet printing of luminescent material, luminescent film and application
CN112251076A
Luminous composition and method for producing organic electroluminescent element
JP2010024407A
Quantum dot light-emitting diode and preparation method therefor
WO2022016822A1