Preparation method of functional aqueous zinc ion battery electrolyte

By adding a selenium crown ether additive with cyano groups to the electrolyte of aqueous zinc-ion batteries, the problems of dendrite growth and hydrogen evolution corrosion of zinc anodes were solved, achieving high-efficiency cycle performance and long life of the batteries, making them suitable for mass production.

CN117691220BActive Publication Date: 2026-11-24NORTHWESTERN POLYTECHNICAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410104832.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2026-11-24
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

Dendrite growth, hydrogen evolution reaction, and corrosion of the zinc anode in aqueous zinc-ion batteries severely affect the battery's cycle performance and lifespan. Existing additives are prone to triggering side reactions in the electrolyte, leading to reduced ion kinetics and decreased electrochemical performance.

Method used

A cyano-containing selenium crown ether additive is mixed with zinc sulfate solution to form a complex, which guides uniform zinc flux, inhibits dendrite growth, and reduces the HOMO energy level of the crown ether through a hydrophobic external framework and electron-withdrawing groups, thereby accelerating ion dynamics, blocking active water molecules from contacting the negative electrode surface, and inhibiting hydrogen evolution and corrosion reactions.

Benefits of technology

It effectively inhibits zinc dendrite growth, improves battery cycle performance and service life, simplifies the manufacturing process, reduces costs, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117691220B_ABST
    Figure CN117691220B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a functional aqueous zinc-ion battery electrolyte, comprising the following steps: S1, preparing a 2 mol / L solution using deionized water and zinc sulfate. ‑1 Zinc sulfate solution; S2, add cyanide-containing selenium crown ether additive to 2 mol L ‑1 A zinc sulfate solution is stirred until homogeneous to obtain a functional aqueous zinc-ion battery electrolyte. This invention employs the above-mentioned method for preparing a functional aqueous zinc-ion battery electrolyte. The crown ether additive can combine with zinc ions to form a complex, guiding a uniform zinc flux and effectively inhibiting dendrite growth. Furthermore, the additive has a hydrophobic external framework, promoting the desolvation of zinc ions. The electron-withdrawing groups (-CN) and selenium in its structure can lower the HOMO energy level of the crown ether, making it easier to donate electrons and accelerating ion dynamics. In addition, the additive blocks the contact between active water molecules and the negative electrode surface, effectively inhibiting side reactions such as hydrogen evolution and corrosion, and improving the battery's cycle performance and service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aqueous zinc-ion battery technology, and in particular to a method for preparing a functional aqueous zinc-ion battery electrolyte. Background Technology

[0002] In recent years, lithium-ion batteries have been considered the most promising electrochemical energy storage devices due to their high energy density, flexibility, and scalability. However, the increasing scarcity of lithium resources and the inherent safety hazards of organic electrolytes have limited their further large-scale application. In contrast, aqueous zinc-ion batteries possess the high energy density of zinc metal (820 mAh·g⁻¹). -1 5855mAh·cm -3 With its low cost (≈$1.35 / lb) and the environmental friendliness and safety of aqueous electrolytes, it is gradually becoming a research hotspot for large-scale power storage systems.

[0003] However, metallic zinc exhibits thermodynamic instability in aqueous electrolytes, easily triggering a series of side reactions that severely restrict the commercialization and large-scale application of aqueous zinc-ion batteries. Specifically, on the one hand, the surface roughness of zinc causes a "sharp effect" during zinc ion deposition, easily leading to uneven zinc flux and uncontrolled dendrite growth. In severe cases, dendrites can pierce the separator, causing battery failure. On the other hand, in conventionally used electrolytes, the zinc ion deposition process is often accompanied by hydrogen evolution reaction, resulting in a local pH increase and the formation of corrosion products such as basic zinc sulfate, which severely deteriorates the battery's cycle performance.

[0004] To address the aforementioned issues, various strategies for suppressing side reactions at the zinc anode have been proposed, including three-dimensional electrode structure design, interface layer modification, and electrolyte additives. Among these, electrolyte additives have attracted widespread attention due to their simple preparation and low cost. Currently, commonly used additives are divided into metal ion additives and organic additives. Both types of additives can be adsorbed onto the zinc anode surface to regulate the deposition behavior of zinc ions. However, the physicochemical properties of these additives differ significantly from those of the electrolyte, easily triggering side reactions during charge and discharge. Furthermore, excessive addition can increase the viscosity of the electrolyte, leading to a decrease in ion kinetics and electrochemical performance. Therefore, rational electrolyte formulation design remains a key issue that urgently needs to be addressed for the commercialization of zinc-ion batteries. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a functional aqueous zinc-ion battery electrolyte. The preparation process is simple and convenient, suitable for large-scale production, and the prepared functional aqueous zinc-ion battery electrolyte can effectively suppress side reactions such as dendrite formation, hydrogen evolution, and corrosion at the zinc anode, thereby greatly improving the battery's service life.

[0006] To achieve the above objectives, the present invention provides a method for preparing a functional aqueous zinc-ion battery electrolyte, comprising the following steps:

[0007] S1. Prepare a 2 mol / L solution using deionized water and zinc sulfate. -1 Zinc sulfate solution;

[0008] S2. Add the cyano-containing selenium crown ether additive to 2 mol L. -1 A zinc sulfate solution was stirred until homogeneous to obtain a functional aqueous zinc-ion battery electrolyte.

[0009] Preferably, the stirring is performed at room temperature, and the stirring time is 2 to 10 hours; more preferably, the stirring time is 6 to 8 hours.

[0010] Preferably, the cyano-containing selenium crown ether additive is mixed with 2 mol L -1 The mass ratio of zinc sulfate solution is (0.001–0.008):1; more preferably, the cyano-containing selenium crown ether additive is mixed with 2 mol / L... -1 The mass ratio of zinc sulfate solution is (0.003~0.006):1; more preferably, the cyano-containing selenium crown ether additive is mixed with 2 mol L... -1 The mass ratio of zinc sulfate solution is 0.005:1.

[0011] A functional aqueous zinc-ion battery includes a positive electrode, a negative electrode, an electrolyte, and a separator between the positive and negative electrodes, wherein the electrolyte is the functional aqueous zinc-ion battery electrolyte prepared in the above steps.

[0012] Therefore, the present invention employs the above-mentioned method for preparing a functional aqueous zinc-ion battery electrolyte, which has the following technical advantages:

[0013] (1) Adding a cyano-containing selenium crown ether additive to a zinc sulfate solution allows the cyano-containing selenium crown ether additive to combine with zinc ions to form a complex, guiding a uniform zinc flux and effectively inhibiting dendrite growth.

[0014] (2) The selenium-containing crown ether additive with cyano group has a hydrophobic external framework, which promotes the desolvation of zinc ions. In addition, the electron-withdrawing group (-CN) in the structure and the selenium element reduce the HOMO energy level of the crown ether, making it easier to donate electrons and accelerate ion dynamics.

[0015] (3) The selenium crown ether additive with cyano group blocks the contact between active water molecules and the negative electrode surface, effectively inhibiting side reactions such as hydrogen evolution and corrosion, and improving the cycle performance and service life of the battery.

[0016] (4) The electrolyte preparation process of this invention is simple, low-cost, and easy to industrialize, and has high application value in the field of aqueous zinc-ion batteries.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0019] Figure 1 The zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 were compared at 1.0 mA cm⁻¹. -2 1.0mAh cm -2 Comparison of cyclic performance under different conditions;

[0020] Figure 2 The zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 were compared at 5.0 mA cm⁻¹. -2 5.0mAh cm -2 Comparison of cyclic performance under different conditions;

[0021] Figure 3 The zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 were compared at 10 mA cm⁻¹. -2 10mAh cm -2 Comparison of cyclic performance under different conditions;

[0022] Figure 4 This is a comparison of the rate performance of the zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 at different current densities.

[0023] Figure 5 Linear sweep scalar (LSV) curves of the zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 are shown.

[0024] Figure 6 The XRD patterns of the zinc electrodes of the zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 after 100 cycles are shown.

[0025] Figure 7 SEM images of the zinc electrode surface morphology of the zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 after 100 cycles.

[0026] Figure 8 This is a light microscope image of the zinc symmetric cell prepared in Example 4 during the zinc deposition process;

[0027] Figure 9 Light microscopy image of the zinc symmetric cell prepared in Comparative Example 1 during the zinc deposition process;

[0028] Figure 10 The desolvation activation energy during the zinc deposition process is compared between the zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1.

[0029] Figure 11 The full cell prepared in Example 4 and the full cell prepared in Comparative Example 1 were compared at 2.0 Ag. -1 Comparison of cycling performance at current density. Detailed Implementation

[0030] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments.

[0031] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.

[0032] Unless otherwise specified, the raw materials used in the following embodiments are all commercially available products in the art.

[0033] Example 1

[0034] A method for preparing a functional aqueous zinc-ion battery electrolyte includes the following steps:

[0035] S1. Weigh 3.67g of zinc sulfate and mix it with 10mL of deionized water, stirring until homogeneous, to obtain 2mol L. -1 Zinc sulfate solution;

[0036] S2. Weigh 0.068g of the cyano-containing selenium crown ether additive and mix it with 2mol L obtained in step (1). -1 The zinc sulfate solution is mixed and stirred on a magnetic stirrer for 8 hours to obtain functional aqueous zinc-ion battery electrolyte A.

[0037] Example 2

[0038] A method for preparing a functional aqueous zinc-ion battery electrolyte includes the following steps:

[0039] S1. Weigh 3.67g of zinc sulfate and mix it with 10mL of deionized water, stirring until homogeneous, to obtain 2mol L. -1 Zinc sulfate solution;

[0040] S2. Weigh 0.041g of the cyano-containing selenium crown ether additive and mix it with the 2mol L obtained in step (1). -1 The zinc sulfate solution is mixed and stirred on a magnetic stirrer for 8 hours to obtain functional aqueous zinc-ion battery electrolyte B.

[0041] Example 3

[0042] A method for preparing a functional aqueous zinc-ion battery electrolyte includes the following steps:

[0043] S1. Weigh 3.67g of zinc sulfate and mix it with 10mL of deionized water, stirring until homogeneous, to obtain 2mol L. -1 Zinc sulfate solution;

[0044] S2. Weigh 0.082g of the cyano-containing selenium crown ether additive and mix it with the 2mol L obtained in step (1). -1 The zinc sulfate solution is mixed and stirred on a magnetic stirrer for 8 hours to obtain functional aqueous zinc-ion battery electrolyte C.

[0045] Example 4

[0046] The preparation of a functional aqueous zinc-ion battery using the functional aqueous zinc-ion battery electrolyte A obtained in Example 1 includes the following steps:

[0047] S1, Zinc Symmetric Battery: Assembled in a 2032-type button cell casing, in the following order: positive electrode casing, zinc electrode sheet, separator, functional aqueous zinc-ion battery electrolyte A, zinc electrode sheet, gasket, spring contact, and negative electrode casing. The assembled battery is placed on a button cell sealing machine and sealed under pressure, then left to stand for 12 hours before electrochemical performance testing.

[0048] S2, Full Cell: Assembled in a 2032-type button cell casing, in the following order: positive electrode casing, positive electrode plate, separator, functional aqueous zinc-ion battery electrolyte A, zinc negative electrode plate, gasket, spring contact, and negative electrode casing. The assembled battery is pressurized and sealed, then left to stand for 12 hours before electrochemical performance testing.

[0049] Comparative Example 1

[0050] An aqueous zinc-ion battery was prepared using the same method as in Example 4, except that the electrolyte used was 2 mol / L. -1 Zinc sulfate solution.

[0051] Electrochemical performance testing

[0052] The batteries assembled in Example 4 and Comparative Example 1 were subjected to constant current charge and discharge tests using the Xinwei Battery Testing System and Chenhua Electrochemical Workstation.

[0053] (1) The zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 were tested using the above-described electrochemical performance testing method at 1.0 mA cm⁻¹. -2 1.0mAh cm -2 5.0mA cm -2 5.0mAh cm-2 ; 10.0mA cm -2 10.0mAh cm -2 Cyclic performance under certain conditions.

[0054] The results are as follows: Figures 1-3 As shown, the battery assembled in Example 4 exhibits better cycle stability compared to Comparative Example 1.

[0055] (2) The rate performance of the zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 were tested using the above electrochemical performance testing method.

[0056] The results are as follows Figure 4 As shown, by changing the current density during cycling, the symmetrical battery assembled in Example 4 exhibits better rate performance than that in Comparative Example 1.

[0057] (3) The linear sweep curves (LSV) of the zinc symmetric cell prepared in Example 4 and the zinc symmetric cell prepared in Comparative Example 1 were detected using the above electrochemical performance detection method.

[0058] The results are as follows Figure 5 As shown, the corrosion potential of Example 4 is more positive and the corrosion current is smaller than that of Comparative Example 1, indicating that the functional aqueous zinc-ion battery electrolyte prepared in Example 1 improves the corrosion resistance of the zinc anode.

[0059] (4) The zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 were tested using the above electrochemical performance testing method after 100 cycles. The XRD patterns of the zinc electrodes in Example 4 and Comparative Example 1 are shown below. Figure 6 As shown.

[0060] It can be seen that obvious basic zinc sulfate byproducts appeared on the surface of the zinc electrode in Comparative Example 1. These byproducts are usually electronically insulating and severely hinder the transport of zinc ions and electrons. However, the zinc electrode surface in Example 4 still showed zinc diffraction peaks similar to the original state, indicating that the corrosion side reaction was effectively suppressed.

[0061] (5) The zinc symmetric battery prepared in Example 4 and the zinc symmetric battery prepared in Comparative Example 1 were tested using the above electrochemical performance testing method after 100 cycles. The SEM images of the zinc electrode surface morphology in Example 4 and Comparative Example 1 are shown below. Figure 7 As shown.

[0062] It can be seen that after 100 cycles, a large number of zinc dendrites appeared on the surface of the zinc electrode in Comparative Example 1, while the surface of the zinc electrode in Example 4 was flat and uniform with no obvious dendrite formation. This indicates that the functional aqueous zinc-ion battery electrolyte prepared in Example 1 can effectively suppress zinc dendrites.

[0063] (6) At 5mA·cm -2 After zinc deposition at the current density for 1 hour, the cross-sectional morphology of the zinc electrode was observed using an optical microscope. The optical micrographs of the zinc electrode in Example 4 and the zinc electrode in Comparative Example 1 during the zinc deposition process are shown below. Figure 8-9 As shown.

[0064] It can be seen that obvious zinc dendrites and bubbles can be seen in the cross section of the zinc electrode in Comparative Example 1, while Example 4 achieves uniform zinc deposition without bubble generation, indicating that the functional aqueous zinc-ion battery electrolyte prepared in Example 1 can effectively suppress dendrite growth and hydrogen evolution reaction.

[0065] (7) The desolvation activation energy was detected using the above electrochemical performance testing method to obtain the functional zinc-ion battery electrolyte prepared in Example 1 and the 2 mol L electrolyte prepared in Comparative Example 1. -1 The desolvation activation energy of zinc sulfate electrolyte during zinc deposition process is as follows: Figure 10 As shown.

[0066] Depend on Figure 10 It can be seen that the impedance and desolvation activation energy of the functional zinc-ion battery electrolyte prepared in Example 1 are significantly lower than those of the 2 mol L⁻¹ electrolyte in Comparative Example 1. -1 The zinc sulfate electrolyte indicates that the functional zinc-ion battery electrolyte prepared in Example 1 is more conducive to accelerating the desolvation and kinetics of zinc ions.

[0067] (8) The electrochemical performance of the full cell prepared in Example 4 and the full cell prepared in Comparative Example 1 were tested using the above-described electrochemical performance testing method at 2.0 Ag. -1 Cyclic performance at current density, results are as follows Figure 11 As shown.

[0068] Depend on Figure 11 It can be seen that, compared with Comparative Example 1, the full cell assembled with the functional zinc-ion battery electrolyte prepared in Example 1 exhibits better cycle stability. This indicates that the functional zinc-ion battery electrolyte prepared in Example 1 can effectively extend the cycle life of the battery.

[0069] Therefore, the present invention employs the above-mentioned method for preparing a functional aqueous zinc-ion battery electrolyte. The prepared functional aqueous zinc-ion battery electrolyte can guide a uniform zinc flux and effectively inhibit dendrite growth. Secondly, the cyano-containing selenium crown ether additive has a hydrophobic external framework, which promotes the desolvation of zinc ions. Furthermore, the electron-withdrawing groups (-CN) and selenium in the structure reduce the HOMO energy level of the crown ether, making it easier to donate electrons and accelerating ion dynamics. Finally, the cyano-containing selenium crown ether additive blocks the contact between active water molecules and the negative electrode surface, effectively inhibiting side reactions such as hydrogen evolution and corrosion, improving the cycle performance and service life of the battery. Moreover, the method provided by the present invention is simple, low-cost, and easy to operate, and can achieve large-scale production.

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a functional aqueous zinc-ion battery electrolyte, characterized in that, Includes the following steps: S1. Prepare a 2 mol / L solution using deionized water and zinc sulfate. -1 Zinc sulfate solution; S2. Add the cyano-containing selenium crown ether additive to 2 mol L. -1 A zinc sulfate solution was stirred until homogeneous to obtain a functional aqueous zinc-ion battery electrolyte.

2. The method for preparing a functional aqueous zinc-ion battery electrolyte according to claim 1, characterized in that: The cyano-containing selenium crown ether additive and 2 mol L -1 The mass ratio of zinc sulfate solution is (0.001~0.008):

1.

3. The method for preparing a functional aqueous zinc-ion battery electrolyte according to claim 2, characterized in that: The cyano-containing selenium crown ether additive and 2 mol L -1 The mass ratio of zinc sulfate solution is (0.003~0.006):

1.

4. The method for preparing a functional aqueous zinc-ion battery electrolyte according to claim 2, characterized in that: The cyano-containing selenium crown ether additive and 2 mol L -1 The mass ratio of zinc sulfate solution is 0.005:

1.

5. The method for preparing a functional aqueous zinc-ion battery electrolyte according to claim 1, characterized in that: The stirring is carried out at room temperature for 2 to 10 hours.

6. A functional aqueous zinc-ion battery, characterized in that: The electrolyte includes a positive electrode, a negative electrode, a separator, and an electrolyte prepared by the method described in any one of claims 1 to 5 for a functional aqueous zinc-ion battery.

Citation Information

Patent Citations

  • Ternary sulfenyl boron trifluoride salt electrolyte as well as preparation method and application thereof

    CN114649571A

  • Aqueous zinc ion electrolyte, zinc ion battery and preparation method thereof

    CN116454418A