Silicon-carbon negative electrode slurry stirring process

By employing a specific step-by-step silicon-carbon anode slurry stirring process in lithium-ion batteries, and utilizing mixed colloid formulations and dispersants under alkaline and acidic conditions, the volume expansion problem of silicon anode materials was solved, improving the cycle performance and dispersion uniformity of the battery, and extending battery life.

CN117695914BActive Publication Date: 2026-11-20MEIZHOU LIANGNENG NEW ENERGY SCI & TECHCO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311794748.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-20
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the volume expansion of silicon anode materials during the lithium insertion/extraction process leads to rapid capacity decay, affecting cycle life. Furthermore, when silicon-carbon materials are mixed with graphite, their conductivity is low, making them prone to electrode powder shedding and agglomeration, which affects battery performance.

Method used

A specific silicon-carbon anode slurry mixing process is employed, which involves preparing a mixed adhesive solution under alkaline and acidic conditions, combining different types of water-based binders and dispersants, and adjusting the stirring speed and temperature to disperse silicon-carbon materials, prevent agglomeration, and improve adhesion and dispersion uniformity.

Benefits of technology

It effectively alleviates electrode powder shedding, improves battery cycle performance, enhances the dispersion uniformity and adhesion of silicon-carbon materials, and extends battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117695914B_ABST
    Figure CN117695914B_ABST
Patent Text Reader

Abstract

The application discloses a silicon-carbon negative electrode slurry stirring process, which adjusts the slurry preparation process, makes the slurry dispersion more uniform, improves the phenomenon of electrode sheet powder falling in the charging and discharging process of silicon-carbon materials, improves the cycle performance of the battery, and meanwhile, the preparation method of the application adopts the dry mixing of powder first, makes the silicon-carbon negative electrode material and the conductive agent more uniformly mixed, and eliminates the agglomeration phenomenon of the silicon-carbon material in the slurry preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery production technology, specifically to the stirring process of silicon-carbon anode slurry. Background Technology

[0002] The current lithium-ion battery anode material—graphite—has reached a specific capacity close to its theoretical value, leaving limited room for further improvement. However, with technological advancements and rising living standards, modern society has a more urgent need for higher energy densities. To increase the energy density of battery cells, it is essential to use anode materials with higher specific capacity and superior performance. Silicon anode materials, due to their high theoretical specific capacity (approaching 4200 mAh / g), have attracted widespread attention and are considered the most promising anode material for improving battery cell energy density. Furthermore, silicon is abundant in the Earth's crust, offering significant development potential. However, the biggest challenge facing silicon anodes is the volume expansion during the lithium insertion / extraction process. This substantial volume expansion leads to rapid capacity decay, significantly reducing cycle life. This large volume expansion also hinders the application and widespread adoption of silicon anode materials in 3C consumer batteries.

[0003] The current conventional method involves mixing silicon and graphite. While ensuring increased capacity, graphite's large specific surface area buffers the expansion and contraction of silicon during charge and discharge. However, silicon-carbon materials have lower conductivity compared to traditional graphite anode materials. Therefore, the uniformity of dispersion of the conductive agent and active material significantly impacts the material's initial efficiency. Furthermore, the significant volume changes during charge and discharge of silicon-carbon materials make them prone to electrode powder shedding, severely affecting cycle life. Agglomeration is also common during slurry preparation. Therefore, the binder, slurry ratio, and slurry preparation process have crucial influences on the electrochemical performance of silicon-carbon materials. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a silicon-carbon anode slurry stirring process. By adjusting the slurry preparation process, the slurry is more evenly dispersed, which improves the electrode powder shedding phenomenon that occurs during the charging and discharging of silicon-carbon materials and improves the cycle performance of the battery.

[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: Design a silicon-carbon anode slurry stirring process, including the following steps: (1) Add alkaline deionized water to mixing tank A and acidic deionized water to mixing tank B; (2) After diluting the water-based adhesive, add it to mixing tank A and mixing tank B at a mass ratio of 1:1, and heat it to 45~55℃ and stir for 2~10 hours. Prepare the adhesive mixture and let it stand for later use. (3) Add the conductive agent to the mixing tank A and stir it while passing in high-temperature circulating water. Mix and stir at a constant temperature of 40℃~50℃ to obtain the prepared adhesive solution A. (4) Add silicon-carbon doped graphite material to the mixing tank B, and simultaneously introduce cooling circulating water. Mix and stir at room temperature (20℃~25℃) to obtain the prepared adhesive solution B. (5) Add the prepared adhesive solutions A and B from steps (3) and (4) into the mixing tank C for mixing, and add the dispersant at the same time. After mixing, a mixed slurry is obtained. (6) Adjust the viscosity of the mixed slurry obtained in step (5), pass the slurry through a 100-300 double-mesh sieve, remove air bubbles to obtain the final slurry.

[0006] Preferably, the weight of deionized water added to the mixing tank A and the mixing tank B in step (1) is the same; the pH value of the deionized water in the mixing tank A is 8-12, and the pH value of the deionized water in the mixing tank B is 2-6.

[0007] Preferably, in step (2), the water-based adhesive is at least one of LA132, LA133, and LA136D. When two water-based adhesives are mixed, their mass ratio is 1:1; when three water-based adhesives are mixed, their mass ratio is 1:1:1; the concentration of the adhesive after dilution is 1.6% to 1.8%; the diluted adhesive is divided into two equal parts and added to mixing tank A and mixing tank B respectively; the concentration of the adhesive solution in mixing tanks A and B is 1.2% to 1.8%.

[0008] Preferably, the conductive agent in step (3) is one or more of Super-P, carbon nanotubes, graphene, Ketjen black, and acetylene black.

[0009] Preferably, the silicon-carbon doped graphite material in step (4) is a mixture of silicon-carbon powder and graphite powder, and the mass ratio of silicon-carbon powder to graphite powder is 1:9 to 3:7.

[0010] Preferably, the dispersant in step (5) is polyethylene glycol 200 or 400 with a molecular weight of 190-420.

[0011] Preferably, the mass ratio of the silicon-carbon doped graphite material, conductive agent, and binder is 80:10:10 to 97:1:2.

[0012] Preferably, in step (5), the weight of the dispersant is 3% to 4.5% of the total weight of the dry materials of the doped graphite material, conductive agent and binder; the dispersant and the mixed adhesive are added simultaneously in 3 to 5 batches. After the first addition, the mixture is stirred at a speed of 1200 to 1500 RPM and 10 to 20 RPM. After each addition, the rotation speed is increased by 5% to 10%. After each addition, the vacuum is evacuated for 3 to 5 minutes, and the vacuum degree is ≤ -0.75 MPa.

[0013] Preferably, in step (6), the viscosity of the slurry is adjusted to 2000-4000 mPa·S.

[0014] Preferably, the mixing speed in steps (3) and (4) is: 1200 RPM to 1500 RPM for rotational mixing and 20-30 RPM for revolution mixing.

[0015] The beneficial effects of this invention are as follows: 1. To address the volume expansion effect of silicon-carbon materials, a mixed adhesive solution of different types of LA water-based binders was formulated. Under alkaline conditions, the functional groups on the carbon black surface were modified into hydroxyl and amine groups, significantly improving hydrophilicity. Simultaneously, under constant temperature conditions, mixing with a hydrophilic binder resulted in more uniform binder dispersion. This effectively improved the adhesion between the coating and foil layers, effectively alleviated electrode powder shedding, and greatly enhanced the battery's cycle performance.

[0016] 2. In an acidic state, the surface of the silicon-carbon material is negatively charged. The repulsion between the silicon-carbon material and the negative charge in the slurry disperses the nano-silicon-carbon particles, preventing their aggregation. Simultaneously, cooling the slurry to room temperature reduces the attraction and mobility between particles, thus preventing aggregation and eliminating the aggregation of silicon-carbon materials during the slurry preparation process, shortening the dispersion time, and improving slurry preparation efficiency.

[0017] 3. By adding the dispersant and the mixed adhesive in multiple steps, the stirring speed, revolution speed and rotation speed are gradually increased in a gradient. Adding too much at once and immediately stirring at high speed will put a large power load on the equipment. This avoids uneven dispersion of the dispersant and also prevents damage to the equipment. Attached Figure Description

[0018] Figure 1 The images show the CPMG-T2 spectrophotometers of the slurry dispersions in the conventional example and the embodiment of the present invention. Detailed Implementation

[0019] The specific embodiments of the present invention are described below with reference to examples. However, these examples are only used to illustrate the present invention in detail and do not limit the scope of the present invention in any way. Unless otherwise specified, the industrial raw materials involved are all commercially available conventional industrial raw materials.

[0020] Example 1: A silicon-carbon anode slurry stirring process, comprising the following steps: (1) Add alkaline deionized water with a pH of 8 to mixing tank A and acidic deionized water with a pH of 2 to mixing tank B; and the weight of deionized water added to mixing tank A and mixing tank B is the same.

[0021] (2) After diluting the water-based adhesive, add it to mixing tank A and mixing tank B at a mass ratio of 1:1. At the same time, heat it to 45~55℃ and stir for 2 hours. Prepare the adhesive mixture and let it stand for later use.

[0022] In this embodiment, the adhesive is a mixture of LA132, LA133 and LA136D water-based adhesives in a mass ratio of 1:1:1. The concentration of the diluted adhesive is 1.6%~1.8%; the diluted adhesive is divided into two equal parts and added to mixing tank A and mixing tank B respectively, and the concentration of the adhesive solution in mixing tanks A and B is 1.2%.

[0023] (3) Add the conductive agent to the mixing tank A and stir, while simultaneously introducing high-temperature circulating water. Mix and stir at a constant temperature of 40°C. The rotation speed of the stirring tank is 1200 RPM, and the revolution speed is 20 RPM. The conductive agent is carbon nanotubes and acetylene black in a mass ratio of 1:1.

[0024] (4) Add silicon-carbon doped graphite material to the mixing tank B, and simultaneously introduce cooling circulating water. Mix and stir at room temperature of 20°C. The rotation speed is 1200 RPM and the revolution speed is 20 RPM. The silicon-carbon doped graphite material is a mixture of silicon-carbon powder and graphite powder, and the mass ratio of silicon-carbon powder to graphite powder is 1:9.

[0025] (5) Add the prepared adhesive solution from steps (3) and (4) to the mixing tank C for mixing, and add a dispersant at the same time. The weight of the dispersant is 3% of the total weight of the dry materials of the doped graphite material, conductive agent and binder. The dispersant and the mixed adhesive solution are added simultaneously in 3 batches. After the first addition, the mixture is stirred at a speed of 1200 RPM and 10 RPM. After each addition, the speed of rotation and revolution is increased by 5% in increments. After each addition, the vacuum is drawn for 3 minutes and the vacuum degree is ≤-0.75 MPa. After the mixing is completed, the mixed slurry is obtained.

[0026] (6) Adjust the viscosity of the mixed slurry obtained in step (5) to 2000 mPa·S, pass the slurry through a 100 double-mesh sieve, remove air bubbles to obtain the final slurry.

[0027] The mass ratio of the silicon-carbon doped graphite material, conductive agent, and binder is 85:5:10; the dispersant is polyethylene glycol 200 or 400 with a molecular weight of approximately 190-420.

[0028] In step (2), the water-based adhesive is at least one of LA132, LA133, and LA136D. When two water-based adhesives are mixed, their mass ratio is 1:1; when three water-based adhesives are mixed, their mass ratio is 1:1:1. Example 2: A silicon-carbon anode slurry stirring process, comprising the following steps: (1) Add alkaline deionized water with a pH of 10 to mixing tank A and acidic deionized water with a pH of 4 to mixing tank B; and the weight of deionized water added to mixing tank A and mixing tank B is the same.

[0029] (2) After diluting the water-based adhesive, add it to mixing tank A and mixing tank B at a mass ratio of 1:1. Heat the mixture to 45~55℃ and stir for 4 hours. Prepare the adhesive mixture and let it stand for later use.

[0030] In this embodiment, the adhesive is a mixture of LA132, LA133, and LA136D water-based adhesives in a mass ratio of 1:1.5:1.5. The concentration of the diluted adhesive is 1.6% to 1.8%. The diluted adhesive is divided into two equal parts and added to mixing tank A and mixing tank B respectively. The concentration of the adhesive solution in mixing tanks A and B is 1.5%.

[0031] (3) Add the conductive agent to the mixing tank A and stir, while simultaneously introducing high-temperature circulating water. Mix and stir at a constant temperature of 45°C. The rotation speed of the stirring tank is 1300 RPM, and the revolution speed is 25 RPM. The conductive agent is Super-P and carbon nanotubes, with a mass ratio of 1:1.

[0032] (4) Add silicon-carbon doped graphite material to mixing tank B, and simultaneously introduce cooling circulating water. Mix and stir at room temperature (25°C) with a rotation speed of 1300 RPM and a revolution speed of 25 RPM. The silicon-carbon doped graphite material is a mixture of silicon-carbon powder and graphite powder, and the mass ratio of silicon-carbon powder to graphite powder is 1.5:8.5.

[0033] (5) Add the prepared adhesive solution from steps (3) and (4) to the mixing tank C for mixing, and add a dispersant at the same time. The weight of the dispersant is 4% of the total weight of the dry materials of the doped graphite material, conductive agent and binder. The dispersant and the mixed adhesive solution are added simultaneously in 4 batches. After the first addition, the mixture is stirred at a speed of 1300 RPM and 15 RPM. After each addition, the speed of rotation and revolution is increased by 6% in increments. After each addition, the vacuum is drawn for 4 minutes and the vacuum degree is ≤-0.75 MPa. After mixing, a mixed slurry is obtained.

[0034] (6) Adjust the viscosity of the mixed slurry obtained in step (5) to 3000 mPa·S, pass the slurry through a 200 double-mesh sieve, remove air bubbles to obtain the final slurry.

[0035] The mass ratio of the silicon-carbon doped graphite material, conductive agent, and binder is 90:5:5; the dispersant is polyethylene glycol 200 or 400 with a molecular weight of approximately 190-420.

[0036] Example 3: A silicon-carbon anode slurry stirring process, comprising the following steps: (1) Add alkaline deionized water with a pH of 12 to mixing tank A and acidic deionized water with a pH of 6 to mixing tank B; and the weight of deionized water added to mixing tank A and mixing tank B is the same.

[0037] (2) After diluting the water-based adhesive, add it to mixing tank A and mixing tank B at a mass ratio of 1:1. At the same time, heat it to 45~55℃ and stir for 2 hours. Prepare the adhesive mixture and let it stand for later use.

[0038] In this embodiment, the adhesive is a mixture of LA132, LA133 and LA136D water-based adhesives in a mass ratio of 1:2:2. The concentration of the diluted adhesive is 1.6%~1.8%; the diluted adhesive is divided into two equal parts and added to mixing tank A and mixing tank B respectively, and the concentration of the adhesive solution in mixing tanks A and B is 1.8%.

[0039] (3) Add the conductive agent to the mixing tank A and stir, while simultaneously introducing high-temperature circulating water. Mix and stir at a constant temperature of 50°C. The rotation speed of the stirring tank is 1500 RPM, and the revolution speed is 30 RPM. The conductive agent is Super-P, carbon nanotubes, and Ketjen Black in a mass ratio of 1:1:1.

[0040] (4) Add silicon-carbon doped graphite material to mixing tank B, and simultaneously introduce cooling circulating water. Mix and stir at room temperature (30°C) with a rotation speed of 1500 RPM and a revolution speed of 30 RPM. The silicon-carbon doped graphite material is a mixture of silicon-carbon powder and graphite powder, and the mass ratio of silicon-carbon powder to graphite powder is 2:8.

[0041] (5) Add the prepared adhesive solution from steps (3) and (4) to the mixing tank C for mixing, and add a dispersant at the same time. The weight of the dispersant is 4% of the total weight of the dry materials of the doped graphite material, conductive agent and binder. The dispersant and the mixed adhesive solution are added simultaneously in 5 batches. After the first addition, the mixing is carried out at a speed of 1500 RPM and 20 RPM. After each addition, the speed of rotation and revolution is increased by 8% in increments. After each addition, the vacuum is drawn for 5 minutes and the vacuum degree is ≤-0.75 MPa. After the mixing is completed, the mixed slurry is obtained.

[0042] (6) Adjust the viscosity of the mixed slurry obtained in step (5) to 4000 mPa·S, pass the slurry through a 300 double-mesh sieve, remove air bubbles to obtain the final slurry.

[0043] The mass ratio of the silicon-carbon doped graphite material, conductive agent, and binder is 90:5:5; the dispersant is polyethylene glycol 200 or 400 with a molecular weight of approximately 190-420; and the binder is a mixture of LA132, LA133, and LA136D water-based binders in a mass ratio of 1:2:2.

[0044] Traditional Example: Following conventional slurry preparation methods, deionized water, binder, conductive agent, and silicon carbide material are sequentially added to a mixing tank and stirred until the viscosity is adjusted to obtain a silicon carbide anode slurry. The spectral peaks of this slurry, compared to those prepared in the example, are measured using a particle surface characteristic analyzer.

[0045] Based on the sample's T2 time, the waiting time TW = 1000ms, and the echo interval TE = 150us. The test results are shown in Table 1 below. T2, T21, and T22 are the peak echo times of the tested spectral peaks, representing the three peaks, with T2 being the dominant peak. The smaller the T2 value of a peak, the narrower the peak width, the larger the signal proportion, indicating better dispersion. A2, A21, and A22 represent the peak distribution, indicating the proportion of the dispersion distributed across the three peaks (signal proportion).

[0046] Table 1

[0047] As can be seen from Table 1, the T2 values ​​in Examples 1 and 2, i.e., the narrow peak width, show that the A2 signal accounts for more than 90%, while the traditional example only accounts for about 60%. This indicates that the dispersion of the slurry is more uniform in the examples of this invention.

[0048] Figure 1 The images show the CPMG-T2 spectra of the slurry dispersions in the conventional example and the embodiment of the present invention. The rightmost peak is the main peak of the dispersion, and its position and signal proportion determine the degree of dispersion. The smaller the T2 value of the main peak, the narrower the peak width, and the larger the signal proportion, the better the dispersibility.

[0049] The present invention has been described in detail above with reference to the embodiments. However, those skilled in the art will understand that, without departing from the spirit of the present invention, various specific parameters in the above embodiments can be changed to form multiple specific embodiments, all of which are common variations of the present invention, and will not be described in detail here.

Claims

1. A stirring process for silicon-carbon anode slurry, characterized in that, Includes the following steps: (1) Add alkaline deionized water to mixing tank A and acidic deionized water to mixing tank B; (2) After diluting the water-based adhesive, add it to mixing tank A and mixing tank B at a mass ratio of 1:1, and heat it to 45~55℃ and stir for 2~10 hours. Prepare the adhesive mixture and let it stand for later use. (3) Add the conductive agent to the mixing tank A and stir it while passing in high-temperature circulating water. Mix and stir at a constant temperature of 40℃~50℃ to obtain the prepared adhesive solution A. (4) Add silicon-carbon doped graphite material to the mixing tank B, and simultaneously introduce cooling circulating water. Mix and stir at room temperature (20℃~25℃) to obtain the prepared adhesive solution B. (5) Add the prepared adhesive solutions A and B from steps (3) and (4) into the mixing tank C for mixing, and add the dispersant at the same time. After mixing, a mixed slurry is obtained. In step (5), the weight of the dispersant is 3% to 4.5% of the total weight of the dry materials of the doped graphite material, conductive agent and binder; the dispersant and the mixed adhesive are added simultaneously in 3 to 5 batches. After the first addition, the mixture is stirred at a speed of 1200 to 1500 RPM and 10 to 20 RPM. After each addition, the rotation speed is increased by 5% to 10%. After each addition, the vacuum is evacuated for 3 to 5 minutes, and the vacuum degree is ≤ -0.75 MPa. (6) Adjust the viscosity of the mixed slurry obtained in step (5), pass the slurry through a 100-300 double-mesh sieve, remove air bubbles to obtain the final slurry.

2. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The weight of deionized water added to the mixing tank A and mixing tank B in step (1) is the same; the pH value of the deionized water in mixing tank A is 8-12, and the pH value of the deionized water in mixing tank B is 2-6.

3. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, In step (2), the water-based adhesive is at least one of LA132, LA133, and LA136D. When two water-based adhesives are mixed, their mass ratio is 1:1; when three water-based adhesives are mixed, their mass ratio is 1:1:1; the concentration of the adhesive after dilution is 1.6% to 1.8%; the diluted adhesive is divided into two equal parts and added to mixing tank A and mixing tank B respectively; the concentration of the adhesive solution in mixing tanks A and B is 1.2% to 1.8%.

4. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The conductive agent in step (3) is one or more of Super-P, carbon nanotubes, graphene, Ketjen black, and acetylene black.

5. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The silicon-carbon doped graphite material in step (4) is a mixture of silicon-carbon powder and graphite powder, and the mass ratio of silicon-carbon powder to graphite powder is 1:9 to 3:

7.

6. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The dispersant in step (5) is polyethylene glycol 200 or 400 with a molecular weight of 190-420.

7. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The mass ratio of the silicon-carbon doped graphite material, conductive agent, and binder is 80:10:10 to 97:1:

2.

8. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, In step (6), the viscosity of the slurry is adjusted to 2000-4000 mPa·S.

9. The silicon-carbon anode slurry stirring process according to claim 1, characterized in that, The mixing speeds in steps (3) and (4) are: rotational mixing speed of 1200 RPM to 1500 RPM and revolution mixing speed of 20-30 RPM.

Citation Information

Patent Citations

  • Silicon-carbon negative electrode material slurry and preparation method thereof

    CN109686979A

  • Preparation method of silicon-carbon negative electrode material of lithium ion battery

    CN109713268A