A perovskite solar cell module encapsulation adhesive film, a preparation method thereof and application thereof
By using a multi-layer polymer encapsulation film design, the problems of acidic substance release and water vapor penetration in perovskite solar cell modules after aging are solved, improving the bonding strength and water vapor barrier performance, and protecting the battery performance.
Patent Information
- Application Number
- CN202311764830.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-19
AI Technical Summary
The encapsulation materials of existing perovskite solar cell modules are prone to producing acidic substances after aging, which affects the bonding strength and water vapor barrier performance. It is impossible to simultaneously improve the bonding strength and reduce the release of acidic substances and the water vapor barrier rate.
The encapsulating film is formed by stacking a multilayer polymer structure, including a silane-modified polyolefin layer, an ethylene-vinyl alcohol copolymer layer, an ethylene-α-olefin copolymer layer, and an ethylene-vinyl acetate copolymer layer in a specific sequence, thereby reducing the release of acidic substances and improving water vapor barrier performance.
It enhances the bonding strength of perovskite solar cell modules, reduces the release of acidic substances, effectively isolates external moisture, and protects cell performance.
Smart Images

Figure CN117701180B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cell module encapsulation, specifically to a perovskite solar cell module encapsulation film, its preparation method, and its application. Background Technology
[0002] Among existing encapsulation materials for perovskite solar cell modules, the residual acids and peroxides in the coating materials have a significant impact on perovskite solar cells. Furthermore, perovskite solar cells are sensitive to moisture barrier properties, thus the encapsulation requirements for perovskite cells are higher than those for crystalline silicon cells. Traditional module encapsulation materials primarily use ethylene vinyl acetate (EVA) as the base resin and peroxides as crosslinking agents. These materials release acidic substances after aging, which corrode the perovskite material and ultimately affect power output. While encapsulation materials using ethylene-octene polymers as the base material and peroxides as crosslinking agents do not produce acidic substances after aging, the decomposition of large amounts of peroxides during lamination still affects the reliability of the perovskite coating, and their moisture barrier performance is also poor. In addition, some peroxide-free thermoplastic polyolefin resins (POE) have the disadvantage of weak adhesion to glass materials. Therefore, finding an encapsulation film material with reliable adhesion, low acid release, and high moisture barrier performance is crucial. Summary of the Invention
[0003] The primary objective of this invention is to address the problem that current encapsulation films for perovskite solar cell modules cannot simultaneously improve adhesive strength, reduce acid release, and enhance water vapor barrier performance. Therefore, this invention proposes an encapsulation film for perovskite solar cell modules that exhibits excellent adhesive strength, low acid release, and high water vapor barrier efficiency.
[0004] The second objective of this invention is to provide a method for preparing the encapsulating film for the above-mentioned perovskite solar cell module.
[0005] A third objective of this invention is to provide the application of the above-mentioned encapsulating film for perovskite solar cell modules in perovskite solar cell modules.
[0006] Specifically, the encapsulating film for the perovskite solar cell module comprises a first polymer layer, a second polymer layer, a third polymer layer, and a fourth polymer layer stacked sequentially; the first polymer layer is a silane-modified polyolefin layer; the second polymer layer is an ethylene-vinyl alcohol copolymer layer; the third polymer layer is an ethylene-α-olefin copolymer layer; and the fourth polymer layer is at least one of a silane-modified polyolefin layer, an ethylene-vinyl acetate copolymer layer, or a mixed layer of ethylene-vinyl acetate copolymer and polyolefin.
[0007] In a preferred embodiment, the thickness of the first polymer layer is 25–100 μm; the thickness of the second polymer layer is 10–50 μm; the thickness of the third polymer layer is 300–400 μm; and the thickness of the fourth polymer layer is 10–100 μm.
[0008] In a preferred embodiment, the first polymer layer contains a polyolefin, a silane coupling agent, and optionally a light stabilizer.
[0009] In a preferred embodiment, based on the total weight of the first polymer layer, the content of the silane-modified polyolefin is 97-99.5 wt%, the content of the silane coupling agent is 0.2-1 wt%, and the content of the light stabilizer is 0-2.5 wt%.
[0010] In a preferred embodiment, the polyolefin is selected from at least one of polyethylene, polypropylene, ethylene-propylene copolymer, α-polyolefin, and ethylene-α-olefin copolymer.
[0011] In a preferred embodiment, the silane coupling agent is selected from at least one of mercaptosilane, epoxysilane, aminosilane, methacryloxysilane, vinylsilane, and isocyanate-based silane.
[0012] In a preferred embodiment, the second polymer layer contains an ethylene-vinyl alcohol copolymer and optionally a light stabilizer.
[0013] In a preferred embodiment, the content of the ethylene-vinyl alcohol copolymer is 98.5 to 99.5 wt%, and the content of the light stabilizer is 0.5 to 1.5 wt%, based on the total weight of the second polymer layer.
[0014] In a preferred embodiment, the ethylene-vinyl alcohol copolymer contains 25-45 wt% ethylene structural units and 55-75 wt% vinyl alcohol structural units.
[0015] In a preferred embodiment, the third polymer layer contains an ethylene-α-olefin copolymer and optionally a light stabilizer.
[0016] In a preferred embodiment, the content of the ethylene-α-olefin copolymer is 97-99 wt%, and the content of the light stabilizer is 1-3 wt%, based on the total weight of the third polymer layer.
[0017] In a preferred embodiment, the ethylene-α-olefin copolymer is selected from at least one of ethylene-butene copolymer, ethylene-hexene copolymer, and ethylene-octene copolymer.
[0018] In a preferred embodiment, the ethylene-α-olefin copolymer contains 60-90 wt% ethylene structural units and 10-40 wt% α-olefin structural units.
[0019] In a preferred embodiment, when the fourth polymer layer is a silane-modified polyolefin layer, the fourth polymer layer contains 97-99.5% polyolefin, 0.2-1 wt% silane coupling agent, and 0-2.5 wt% light stabilizer, based on the total weight of the fourth polymer layer.
[0020] In a preferred embodiment, when the fourth polymer layer is an ethylene-vinyl acetate copolymer layer, the fourth polymer layer contains, based on the total weight of the fourth polymer layer, 91-99 wt% ethylene-vinyl acetate copolymer, 0.01-0.4 wt% peroxide, 0.1-2 wt% acid neutralizer, 0.5-5 wt% silane coupling agent, and 0-2 wt% light stabilizer.
[0021] In a preferred embodiment, when the fourth polymer layer is a mixture of ethylene-vinyl acetate copolymer and polyolefin, the fourth polymer layer contains, based on the total weight of the fourth polymer layer, 33-65 wt% ethylene-vinyl acetate copolymer, 33-65 wt% polyolefin, 0.01-0.4 wt% peroxide, 0.1-2 wt% acid neutralizer, 0.5-5 wt% silane coupling agent, and 0-2% light stabilizer.
[0022] In a preferred embodiment, the mass ratio of the ethylene vinyl acetate copolymer to the polyolefin is 1:(0.5 to 1.5).
[0023] In a preferred embodiment, the ethylene-vinyl acetate copolymer contained in the fourth polymer layer contains 65-90 wt% ethylene structural units and 10-35 wt% vinyl acetate structural units.
[0024] In a preferred embodiment, the polyolefin contained in the fourth polymer layer is selected from at least one of polyethylene, polypropylene, ethylene-propylene copolymer, α-polyolefin and ethylene-α-olefin copolymer.
[0025] In a preferred embodiment, the acid neutralizer is selected from at least one of magnesium stearate, zinc stearate, and calcium stearate.
[0026] In a preferred embodiment, the silane coupling agent contained in the fourth polymer layer is selected from at least one of mercaptosilane, epoxysilane, aminosilane, methacryloxysilane, vinylsilane, and isocyanate-based silane.
[0027] In a preferred embodiment, the encapsulating film of the perovskite solar cell module further includes a fifth polymer layer located between the third polymer layer and the fourth polymer layer, wherein the fifth polymer layer is an ethylene-vinyl alcohol copolymer layer.
[0028] In a preferred embodiment, the fifth polymer layer contains an ethylene-vinyl alcohol copolymer and optionally a light stabilizer.
[0029] In a preferred embodiment, the content of the ethylene-vinyl alcohol copolymer is 98.5 to 99.5 wt%, and the content of the light stabilizer is 0.5 to 1.5 wt%, based on the total weight of the fifth polymer layer.
[0030] In a preferred embodiment, the ethylene-vinyl alcohol copolymer contains 25-45 wt% ethylene structural units and 55-75 wt% vinyl alcohol structural units.
[0031] In a preferred embodiment, the thickness of the fifth polymer layer is 10–50 μm.
[0032] The method for preparing the encapsulating film for perovskite solar cell modules provided by the present invention includes mixing the raw materials required for the first polymer layer, the second polymer layer, the third polymer layer, the fourth polymer layer, and optionally the fifth polymer layer evenly, adding them to an extruder, setting the extrusion temperature of each layer, and casting them through the same die according to the preset thickness of each layer to obtain the encapsulating film for perovskite solar cell modules.
[0033] In a preferred embodiment, the extrusion temperature of the first polymer layer is 140–180°C.
[0034] In a preferred embodiment, the extrusion temperature of the second polymer layer is 160–180°C.
[0035] In a preferred embodiment, the extrusion temperature of the third polymer layer is 140–160°C.
[0036] In a preferred embodiment, the extrusion temperature of the fourth polymer layer is 80–180°C.
[0037] In a preferred embodiment, the extrusion temperature of the fifth polymer layer is 160–180°C.
[0038] The key to this invention lies in layering a silane-modified polyolefin layer, an ethylene-vinyl alcohol copolymer layer, an ethylene-α-olefin copolymer layer, a silane-modified polyolefin layer / ethylene-vinyl acetate copolymer layer / ethylene-vinyl acetate copolymer and a polyolefin mixture layer in a specific order to form a perovskite solar cell module encapsulation film. This not only reduces the release of acidic substances from the encapsulation film, preventing them from affecting the performance of the perovskite solar cell, but also improves the bonding strength and effectively isolates external moisture, reducing the impact of moisture on the perovskite solar cell. Attached Figure Description
[0039] Figure 1 This is a schematic diagram of the structure of the encapsulating film prepared in Example 1.
[0040] Figure 2 This is a schematic diagram of the structure of the encapsulating film prepared in Example 2.
[0041] Figure 3 This is a schematic diagram of the structure of the encapsulating film prepared in Example 3.
[0042] Figure 4 This is a schematic diagram of the structure of the encapsulating film prepared in Example 4.
[0043] Figure 5 This is a schematic diagram of the structure of the encapsulating film prepared in Examples 5 and 6.
[0044] Figure 6 This is a schematic diagram of the structure of the encapsulating film prepared in Example 1 when it is used in a perovskite solar cell. Detailed Implementation
[0045] The perovskite solar cell module encapsulation film provided by this invention comprises a first polymer layer, a second polymer layer, a third polymer layer, and a fourth polymer layer stacked sequentially. The first polymer layer is a silane-modified polyolefin layer; the second polymer layer is an ethylene-vinyl alcohol copolymer layer; the third polymer layer is an ethylene-α-olefin copolymer layer; and the fourth polymer layer is at least one of a silane-modified polyolefin layer, an ethylene-vinyl acetate copolymer layer, or a mixture of an ethylene-vinyl acetate copolymer and a polyolefin. Furthermore, the perovskite solar cell module encapsulation film preferably further includes a fifth polymer layer, which is located between the third and fourth polymer layers, and this fifth polymer layer is an ethylene-vinyl alcohol copolymer layer.
[0046] In this invention, the thickness of the encapsulating film for the perovskite solar cell module is preferably 450–550 μm, such as 450 μm, 460 μm, 470 μm, 480 μm, 490 μm, 500 μm, 510 μm, 520 μm, 530 μm, 540 μm, 550 μm, or any value between them. The thickness of the first polymer layer is preferably 25–100 μm, such as 25 μm, 28 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value between them. The thickness of the second polymer layer is preferably 10–50 μm, such as 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, or any value between them. The thickness of the third polymer layer is preferably 300–400 μm, such as 300 μm, 310 μm, 320 μm, 330 μm, 340 μm, 350 μm, 360 μm, 370 μm, 380 μm, 390 μm, 400 μm, or any value between them. The thickness of the fourth polymer layer is preferably 10–100 μm, such as 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value between them. The thickness of the fifth polymer layer is preferably 10–50 μm, such as 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, or any value between them.
[0047] In this invention, the first polymer layer preferably contains a polyolefin, a silane coupling agent, and optionally a light stabilizer. Based on the total weight of the first polymer layer, the polyolefin content is preferably 97–99.5 wt%, such as 97.2 wt%, 97.5 wt%, 97.8 wt%, 98 wt%, 98.2 wt%, 98.5 wt%, 98.8 wt%, 99 wt%, 99.2 wt%, 99.5 wt%, or any value between therewith. The silane coupling agent content is preferably 0.2–1 wt%, such as 0.2 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, or any value between therewith. The light stabilizer content is preferably 0–2.5 wt%, such as 0 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.5 wt%, or any value between therewith.
[0048] In this invention, the second polymer layer preferably contains an ethylene-vinyl alcohol copolymer and, optionally, a light stabilizer. Based on the total weight of the second polymer layer, the content of the ethylene-vinyl alcohol copolymer is preferably 98.5–99.5 wt%, such as 98.5 wt%, 98.8 wt%, 99 wt%, 99.2 wt%, 99.5 wt%, or any value between therewith. The content of the light stabilizer is preferably 0.5–1.5 wt%, such as 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, or any value between therewith. The content of ethylene structural units in the ethylene-vinyl alcohol copolymer is preferably 25–45 wt%, such as 25 wt%, 28 wt%, 30 wt%, 32 wt%, 35 wt%, 38 wt%, 40 wt%, 42 wt%, 45 wt%, or any value between therewith. The content of vinyl alcohol structural units in the ethylene-vinyl alcohol copolymer is preferably 55-75 wt%, such as 55 wt%, 58 wt%, 60 wt%, 62 wt%, 65 wt%, 68 wt%, 70 wt%, 72 wt%, 75 wt%, or any value between them.
[0049] In this invention, the third polymer layer preferably contains an ethylene-α-olefin copolymer and optionally a light stabilizer. Based on the total weight of the third polymer layer, the content of the ethylene-α-olefin copolymer is preferably 97–99 wt%, such as 97 wt%, 97.2 wt%, 97.5 wt%, 97.8 wt%, 98 wt%, 98.2 wt%, 98.5 wt%, 98.8 wt%, 99 wt%, or any value between therewith. The content of the light stabilizer is 1–3 wt%, such as 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.5 wt%, 3 wt%, or any value between therewith. The ethylene-α-olefin copolymer is preferably selected from at least one of ethylene-butene copolymer, ethylene-hexene copolymer, and ethylene-octene copolymer. The ethylene structural unit content in the ethylene-α-olefin copolymer is 60–90 wt%, such as 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or any value between these values. The α-olefin structural unit content in the ethylene-α-olefin copolymer is 10–40 wt%, such as 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, or any value between these values.
[0050] In this invention, when the fourth polymer layer is preferably a silane-modified polyolefin layer, based on the total weight of the fourth polymer layer, the fourth polymer layer preferably contains polyolefin, a silane coupling agent, and optionally a light stabilizer. The polyolefin content is preferably 97-99.5%, such as 97.wt%, 97.2wt%, 97.5wt%, 97.8wt%, 98wt%, 98.2wt%, 98.5wt%, 98.8wt%, 99wt%, 99.2wt%, 99.5wt%, or any value between them. The silane coupling agent content is preferably 0.2-1wt%, such as 0.2wt%, 0.5wt%, 0.8wt%, 1wt%, or any value between them. The content of the light stabilizer is preferably 0 to 2.5 wt%, such as 0 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.2 wt%, 2.5 wt%, or any value between them.
[0051] In this invention, when the fourth polymer layer is preferably an ethylene-vinyl acetate copolymer layer, based on the total weight of the fourth polymer layer, the fourth polymer layer preferably contains ethylene-vinyl acetate copolymer, peroxide, acid neutralizer, silane coupling agent, and optionally a light stabilizer. The content of the ethylene-vinyl acetate copolymer is preferably 91-99 wt%, such as 91 wt%, 92 wt%, 93 wt%, 94 wt%, 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%, or any value between therewith. The content of the peroxide is preferably 0.01-0.4 wt%, such as 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, or any value between therewith. The content of the acid neutralizing agent is preferably 0.1–2 wt%, such as 0.1 wt%, 0.5 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, or any value between them. The content of the silane coupling agent is preferably 0.5–5 wt%, such as 0.5 wt%, 0.8 wt%, 1 wt%, 2 wt%, 5 wt%, or any value between them. The content of the light stabilizer is preferably 0–2 wt%, such as 0 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, or any value between them.
[0052] In this invention, when the fourth polymer layer is preferably a mixed copolymer layer of ethylene-vinyl acetate copolymer and polyolefin, based on the total weight of the fourth polymer layer, the fourth polymer layer preferably contains ethylene-vinyl acetate copolymer, polyolefin, peroxide, acid neutralizer, silane coupling agent, and optionally a light stabilizer. The content of the ethylene-vinyl acetate copolymer is preferably 33-65 wt%, such as 33 wt%, 35 wt%, 38 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, or any value between therewith. The content of the polyolefin is preferably 33-65 wt%, such as 33 wt%, 35 wt%, 38 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, or any value between therewith. The content of the peroxide is preferably 0.01-0.4 wt%. The content of the acid neutralizer is preferably 0.1-2 wt%. The content of the silane coupling agent is preferably 0.5–5 wt%. The content of the light stabilizer is preferably 0–2 wt%.
[0053] In this invention, the mass ratio of ethylene vinyl acetate to polyolefin is preferably 1:(0.5-1.5), such as 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, or any value between them. The content of ethylene structural units in the ethylene-vinyl acetate copolymer contained in the fourth polymer layer is preferably 65-90 wt%, such as 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or any value between them, and the content of vinyl acetate structural units is preferably 10-35 wt%, such as 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or any value between them.
[0054] In this invention, the polyolefins in the first polymer layer and the fourth polymer layer are each independently preferably selected from at least one of polyethylene, polypropylene, ethylene-propylene copolymer, α-polyolefin and ethylene-α-olefin copolymer. The silane coupling agents in the first polymer layer and the fourth polymer layer are each independently preferably selected from at least one of mercaptosilane, epoxysilane, aminosilane, methacryloyloxysilane, vinylsilane, and isocyanate-based silane. Specific examples include, but are not limited to, γ-(methacryloyloxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-epoxypropoxypropyltrimethoxysilane, 3-epoxypropoxypropylmethyldimethoxysilane, 3-epoxypropoxypropylmethyldiethoxysilane, 3-epoxypropoxypropylmethyldiethoxysilane, 3-epoxypropoxypropylmethyldiethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 203-(meth)acryloyloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and 3-isocyanate-propyltrimethoxysilane.
[0055] The peroxide may be selected from at least one of cumene peroxide, di-tert-butylperoxide, di-isopropylbenzene hydroperoxide, 2,5-dimethyl-2,5-di-tert-butylperoxide, 4,4-di(tert-amylperoxy)valerate, tert-butyl peroxide-2-ethylhexyl carbonate (TBEC), ethyl 3,3-di(tert-butylperoxy)butyrate, tert-amyl peroxide-2-ethylhexyl carbonate, and 1,1-bis(tert-amylperoxy)cyclohexane. The acid neutralizing agent is preferably selected from at least one of magnesium stearate, zinc stearate, and calcium stearate.
[0056] In this invention, the fifth polymer layer preferably contains an ethylene-vinyl alcohol copolymer and, optionally, a light stabilizer. Based on the total weight of the fifth polymer layer, the content of the ethylene-vinyl alcohol copolymer is 98.5–99.5 wt%, such as 98.5 wt%, 98.8 wt%, 99 wt%, 99.2 wt%, 99.5 wt%, or any value between therewith. The content of the light stabilizer is preferably 0.5–1.5 wt%, such as 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, or any value between therewith. The content of ethylene structural units in the ethylene-vinyl alcohol copolymer is preferably 25–45 wt%, such as 25 wt%, 28 wt%, 30 wt%, 32 wt%, 35 wt%, 38 wt%, 40 wt%, 42 wt%, 45 wt%, or any value between therewith. The content of vinyl alcohol structural units in the ethylene-vinyl alcohol copolymer is preferably 55-75 wt%, such as 55 wt%, 58 wt%, 60 wt%, 62 wt%, 65 wt%, 68 wt%, 70 wt%, 72 wt%, 75 wt%, or any value between them.
[0057] In this invention, the light stabilizers contained in the first polymer layer, second polymer layer, third polymer layer, fourth polymer layer, and fifth polymer layer are preferably each independently selected from at least one of benzotriazoles, octyltriazinones, benzophenones, and hindered amines. The benzotriazole light stabilizer may be selected from at least one of 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol (UV-234), 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (UV-326), 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole (UV-327), 2-(2H-benzotriazole-2-yl)-4,6-di-tert-pentylphenol (UV-328), and 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole (UV-329). The benzophenone-based light stabilizer may be 2-hydroxy-4-n-octyloxybenzophenone (UV-531) and / or 2-hydroxy-4-methoxybenzophenone (UV-9). The hindered amine-based light stabilizer may be poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol) ester (light stabilizer 622) and / or bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (light stabilizer 770).
[0058] In this invention, the method for preparing the encapsulating film for a perovskite solar cell module includes mixing the raw materials required for a first polymer layer, a second polymer layer, a third polymer layer, a fourth polymer layer, and optionally a fifth polymer layer, and then adding them to an extruder. The extrusion temperature of each layer is set, and the layers are cast through a single die according to a preset thickness to obtain the encapsulating film for the perovskite solar cell module. The raw materials include the polymers required for each layer and corresponding additives such as light stabilizers. Furthermore, in a specific embodiment, the raw materials for forming the polymers of each layer (resin, silane coupling agent, initiator, co-crosslinking agent, etc.) and corresponding additives such as light stabilizers can be directly added to the extruder. During extrusion, due to the high temperature, the raw materials for forming the polymers will react in situ to generate the corresponding polymers, ultimately obtaining the target component. Additionally, the extrusion temperature of the first polymer layer is preferably 140–180°C, such as 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, or any value between them. The extrusion temperature of the second polymer layer is preferably 160–180°C, such as 160°C, 162°C, 165°C, 168°C, 170°C, 172°C, 175°C, 178°C, 180°C, or any value between them. The extrusion temperature of the third polymer layer is preferably 140–160°C, such as 140°C, 142°C, 145°C, 148°C, 150°C, 152°C, 155°C, 158°C, 160°C, or any value between them. The extrusion temperature of the fourth polymer layer is preferably 80–180°C, such as 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C, 98°C, 100°C, 120°C, 150°C, 180°C, or any value between them. The extrusion temperature of the fifth polymer layer is preferably 160-180°C, such as 160°C, 162°C, 165°C, 168°C, 170°C, 172°C, 175°C, 178°C, 180°C or any value between them.
[0059] The present invention will be described in detail below through specific embodiments.
[0060] The raw materials used in the following examples and comparative examples are as follows: polyolefin (ethylene-α-octene copolymer, ethylene to α-octene content ratio of 75:25), purchased from Mitsui Chemicals, Ltd., brand name TAFMER DF740; polyolefin, purchased from Evonik Specialty Chemicals (Shanghai) Co., Ltd., brand name VESTOPLAST 206; ethylene-vinyl alcohol copolymer (ethylene to vinyl alcohol content ratio of 44:56), purchased from Changchun Petrochemical Co., Ltd., brand name EVASIN EV4405 V / F; ethylene-ethyl acetate copolymer (ethylene to vinyl acetate content ratio of 72:28), purchased from Samsung Total, brand name EVA PV280; ethylene-α-octene copolymer (ethylene to α-octene content ratio of 70:30), purchased from Dow Chemical, USA, brand name POE PV8660.
[0061] Example 1: Preparation of encapsulating film for perovskite solar cell modules
[0062] First polymer layer: 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531) and 0.4 wt% light stabilizer (Tinuvin 622).
[0063] Second polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0064] The third polymer layer consists of 98.6 wt% ethylene-α-octene copolymer (TAFMER DF740), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0065] Fifth polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0066] Fourth polymer layer: 99 wt% ethylene-ethyl acetate copolymer (EVA PV280), 0.2 wt% peroxide (TBEC), 0.1 wt% acid neutralizer (magnesium stearate) and 0.7 wt% silane coupling agent (KBM503).
[0067] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperatures to 160℃, 170℃, 160℃, 170℃, and 90℃ respectively. Then, according to... Figure 1 The 5-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 300μm, 25μm, and 100μm respectively, can be obtained by casting with the same die to produce a product with... Figure 1 The encapsulation film with the structure shown.
[0068] Example 2: Preparation of encapsulating film for perovskite solar cell modules
[0069] First polymer layer: 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531) and 0.4 wt% light stabilizer (Tinuvin 622).
[0070] Second polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0071] The third polymer layer consists of 98.6 wt% ethylene-α-octene copolymer (TAFMER DF740), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0072] Fifth polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0073] The fourth polymer layer consists of 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0074] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperature to 160℃, 170℃, 160℃, 170℃, and 160℃ respectively. Then, according to... Figure 2The 5-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 300μm, 25μm, and 100μm respectively, can be obtained by casting with the same die to produce a product with... Figure 2 The encapsulation film with the structure shown.
[0075] Example 3: Preparation of encapsulating film for perovskite solar cell modules
[0076] First polymer layer: 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531) and 0.4 wt% light stabilizer (Tinuvin 622).
[0077] Second polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0078] The third polymer layer consists of 98.6 wt% ethylene-α-octene copolymer (TAFMER DF740), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0079] The fourth polymer layer consists of 66 wt% ethylene-ethyl acetate copolymer (EVA PV280), 33 wt% ethylene-α-octene copolymer (POE PV8660), 0.2 wt% peroxide (TBEC), 0.1 wt% acid neutralizer (zinc stearate), and 0.7 wt% silane coupling agent (KBM503).
[0080] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperatures to 160℃, 170℃, 140℃, and 90℃ respectively. Then, according to... Figure 3 The four-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 325μm, and 100μm respectively, can be obtained by casting with the same die to produce a product with... Figure 3 The encapsulation film with the structure shown.
[0081] Example 4: Preparation of encapsulating film for perovskite solar cell modules
[0082] First polymer layer: 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531) and 0.4 wt% light stabilizer (Tinuvin 622).
[0083] Second polymer layer: 99 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0084] The third polymer layer consists of 98.6 wt% ethylene-α-octene copolymer (TAFMER DF740), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0085] The fourth polymer layer consists of 50 wt% ethylene-α-octene copolymer (TAFMER DF740), 47.8 wt% polyolefin (VESTOPLAST 206), 0.8 wt% silane coupling agent (KBM503), 1 wt% light stabilizer (UV531), and 0.4 wt% light stabilizer (Tinuvin 622).
[0086] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperature to 160℃, 170℃, 160℃, and 160℃ respectively. Then, according to... Figure 4 The four-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 375μm, and 50μm respectively, can be obtained by casting with the same die to produce a product with... Figure 4 The encapsulation film with the structure shown.
[0087] Example 5: Preparation of encapsulating film for perovskite solar cell modules
[0088] First polymer layer: 43 wt% ethylene-α-octene copolymer (TAFMER DF740), 54.3 wt% polyolefin (VESTOPLAST 206), 0.2 wt% silane coupling agent (KBM503), 1.3 wt% light stabilizer (UV531) and 1.2 wt% light stabilizer (Tinuvin 622).
[0089] Second polymer layer: 99.5 wt% ethylene-vinyl alcohol copolymer, 0.2 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0090] The third polymer layer consists of 97 wt% ethylene-α-octene copolymer (TAFMER DF740), 1.5 wt% light stabilizer (UV531), and 1.5 wt% light stabilizer (Tinuvin 622).
[0091] Fifth polymer layer: 99.5 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.2 wt% light stabilizer (UV531) and 0.3 wt% light stabilizer (Tinuvin 622).
[0092] Fourth polymer layer: 92.6 wt% ethylene-ethyl acetate copolymer (EVA PV280), 0.4 wt% peroxide (TBEC), 2 wt% acid neutralizer (magnesium stearate) and 5 wt% silane coupling agent (KBM503).
[0093] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperatures to 180℃, 160℃, 140℃, 160℃, and 180℃ respectively. Then, according to... Figure 5 The 5-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 300μm, 25μm, and 100μm respectively, can be obtained by casting with the same die to produce a product with... Figure 2 The encapsulation film with the structure shown.
[0094] Example 6: Preparation of encapsulating film for perovskite solar cell modules
[0095] First polymer layer: 45 wt% ethylene-α-octene copolymer (TAFMER DF740), 54.3 wt% polyolefin (VESTOPLAST 206), 0.6 wt% silane coupling agent (KBM503) and 0.1 wt% light stabilizer (Tinuvin 622).
[0096] Second polymer layer: 98.5 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.8 wt% light stabilizer (Tinuvin 622).
[0097] The third polymer layer consists of 99 wt% ethylene-α-octene copolymer (TAFMER DF740), 0.3 wt% light stabilizer (UV531), and 0.7 wt% light stabilizer (Tinuvin 622).
[0098] Fifth polymer layer: 98.5 wt% ethylene-vinyl alcohol copolymer (EVASIN EV4405 V / F), 0.7 wt% light stabilizer (UV531) and 0.8 wt% light stabilizer (Tinuvin 622).
[0099] The fourth polymer layer consists of 33 wt% ethylene-ethyl acetate copolymer (EVA PV280), 66 wt% ethylene-α-octene copolymer (POE PV8660), 0.2 wt% peroxide (TBEC), 0.1 wt% acid neutralizer (zinc stearate), and 0.7 wt% silane coupling agent (KBM503).
[0100] After thoroughly mixing the above-mentioned materials, pour them sequentially into the extruder for later use. Set the die exit temperature to 140℃, 140℃, 180℃, 140℃, and 140℃ respectively. Then, according to... Figure 5 The 5-layer structure shown, with each layer having thicknesses of 50μm, 25μm, 300μm, 25μm, and 100μm respectively, can be obtained by casting with the same die to produce a product with... Figure 2 The encapsulation film with the structure shown.
[0101] Comparative Example 1
[0102] EVA encapsulation film commonly used in existing technologies.
[0103] Comparative Example 2
[0104] The encapsulating film for perovskite solar cell modules was prepared according to the method of Example 1, except that the first polymer layer was not included, and the thickness of the second polymer layer was increased to 75 μm. Specifically:
[0105] The materials forming the second, third, fifth, and fourth polymer layers are mixed and poured sequentially into an extruder for later use. The die exit temperatures are set to 170℃, 160℃, 170℃, and 90℃, respectively. Then, based on the four-layer structure, with each layer having a thickness of 75μm, 300μm, 25μm, and 100μm, respectively, the reference encapsulation film is obtained by casting through the same die.
[0106] Comparative Example 3
[0107] The encapsulating film for perovskite solar cell modules was prepared according to the method of Example 3, except that the second polymer layer was not included, and the thickness of the first polymer layer was increased to 75 μm. Specifically:
[0108] The materials forming the first, third, and fourth polymer layers are mixed and poured into an extruder in sequence. The die exit temperatures are set to 160°C, 140°C, and 90°C, respectively. Then, based on the three-layer structure and with each layer having a thickness of 75μm, 325μm, and 100μm, respectively, the reference encapsulation film is obtained by casting through the same die.
[0109] Test case
[0110] The encapsulating films of the above embodiments and comparative examples were prepared according to... Figure 6 The structure shown is assembled into a perovskite solar cell structure, wherein the thickness of the glass layers on both sides is 3.2 mm, the thickness of the perovskite layer is 500 nm, and the thickness of the encapsulating film layer is 500 μm. Its performance is then tested according to the following method.
[0111] (1) Water vapor transmission rate test: Select a film with a thickness of 500μm (control the thickness deviation within ±10μm), and then use the MOCON water vapor barrier instrument. Set the instrument test temperature to 38℃ and the humidity to 90%, and then calculate the weight of water vapor transmitted per unit square meter in 1 day. The results are shown in Table 1.
[0112] (2) Adhesion test: The laminator was set to a temperature of about 125℃. The glass layer, perovskite layer, encapsulating film layer and glass layer were stacked in sequence. The first polymer layer of the encapsulating film layer was bonded to the perovskite layer. The lamination was then carried out for 20 minutes. After cooling to room temperature, the layers were placed under a humidity of 85% for 24 hours. The peel force of the encapsulating film layer on the perovskite layer and the glass layer was then tested. The results are shown in Table 1.
[0113] (3) Acid release: The encapsulating film was placed between two layers of PTFE cloth, hot-pressed at 125°C for 30 min, and then refluxed in xylene solvent at 60°C for 48 h. The pH value was then tested, and the results are shown in Table 1.
[0114] Table 1
[0115]
[0116]
[0117] Compared to the commonly used EVA encapsulating film in Comparative Example 1, the encapsulating film provided in this embodiment of the invention has lower water vapor permeability and less acidic substance release. A comparison of Example 1 with Comparative Examples 2 and 3 shows that without a silane-modified polyolefin layer or an ethylene-vinyl alcohol copolymer layer, either the adhesive strength or the water vapor barrier performance will decrease; both cannot be achieved simultaneously. In summary, the encapsulating film provided by this invention combines low water vapor permeability and high adhesive strength, and can reduce the release of acidic substances, thus preventing them from affecting the performance of perovskite solar cells.
[0118] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention.
Claims
1. A perovskite solar cell module encapsulation film, characterized in that, The encapsulating film for the perovskite solar cell module comprises a first polymer layer, a second polymer layer, a third polymer layer, a fifth polymer layer, and a fourth polymer layer stacked sequentially. The first polymer layer is a silane-modified polyolefin layer; the second polymer layer is an ethylene-vinyl alcohol copolymer layer; the third polymer layer is an ethylene-α-olefin copolymer layer; the fifth polymer layer is an ethylene-vinyl alcohol copolymer layer; the fourth polymer layer is a silane-modified polyolefin layer or a mixture of ethylene-vinyl acetate copolymer and polyolefin. When the fourth polymer layer is a mixture of ethylene-vinyl acetate copolymer and polyolefin, the mass ratio of ethylene-vinyl acetate to polyolefin is 1:
2. The thickness of the first polymer layer is 25~100μm; the thickness of the second polymer layer is 10~50μm; the thickness of the third polymer layer is 300~400μm; the thickness of the fifth polymer layer is 10~50μm; and the thickness of the fourth polymer layer is 10~100μm.
2. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, The first polymer layer contains a polyolefin, a silane coupling agent, and an optional light stabilizer.
3. The encapsulating film for a perovskite solar cell module according to claim 2, characterized in that, Based on the total weight of the first polymer layer, the content of the polyolefin is 97~99.5wt%, the content of the silane coupling agent is 0.2~1wt%, and the content of the light stabilizer is 0~2.2wt%.
4. The encapsulating film for a perovskite solar cell module according to claim 2, characterized in that, The polyolefin is selected from at least one of polyethylene, polypropylene, and ethylene-propylene copolymer.
5. The encapsulating film for a perovskite solar cell module according to claim 2, characterized in that, The silane coupling agent is selected from at least one of mercaptosilane, epoxysilane, aminosilane, methacryloxysilane, vinylsilane, and isocyanate-based silane.
6. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, The second polymer layer contains an ethylene-vinyl alcohol copolymer and an optional light stabilizer.
7. The encapsulating film for a perovskite solar cell module according to claim 6, characterized in that, Based on the total weight of the second polymer layer, the content of the ethylene-vinyl alcohol copolymer is 98.5~99.5 wt%, and the content of the light stabilizer is 0.5~1.5 wt%.
8. The encapsulating film for a perovskite solar cell module according to claim 6, characterized in that, The ethylene-vinyl alcohol copolymer contains 25-45 wt% ethylene structural units and 55-75 wt% vinyl alcohol structural units.
9. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, The third polymer layer contains an ethylene-α-olefin copolymer and an optional light stabilizer.
10. The encapsulating film for a perovskite solar cell module according to claim 9, characterized in that, Based on the total weight of the third polymer layer, the content of the ethylene-α-olefin copolymer is 97-99 wt%, and the content of the light stabilizer is 1-3 wt%.
11. The encapsulating film for a perovskite solar cell module according to claim 9, characterized in that, The ethylene-α-olefin copolymer is selected from at least one of ethylene-butene copolymer, ethylene-hexene copolymer, and ethylene-octene copolymer.
12. The encapsulating film for a perovskite solar cell module according to claim 9, characterized in that, The ethylene-α-olefin copolymer contains 60-90 wt% ethylene structural units and 10-40 wt% α-olefin structural units.
13. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, When the fourth polymer layer is a silane-modified polyolefin layer, based on the total weight of the fourth polymer layer, the fourth polymer layer contains 97-99.5% polyolefin, 0.2-1 wt% silane coupling agent, and 0-2.2 wt% light stabilizer.
14. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, When the fourth polymer layer is a mixture of ethylene-vinyl acetate copolymer and polyolefin, based on the total weight of the fourth polymer layer, the fourth polymer layer contains 33-65 wt% ethylene-vinyl acetate copolymer, 66 wt% polyolefin, 0.01-0.4 wt% peroxide, 0.1-2 wt% acid neutralizer, 0.5-5 wt% silane coupling agent, and 0-2 wt% light stabilizer, and the sum of the mass percentages of each component satisfies 100%.
15. The encapsulating film for a perovskite solar cell module according to claim 14, characterized in that, The ethylene-vinyl acetate copolymer contained in the fourth polymer layer contains 65-90 wt% ethylene structural units and 10-35 wt% vinyl acetate structural units.
16. The encapsulating film for a perovskite solar cell module according to claim 13 or 14, characterized in that, The polyolefin contained in the fourth polymer layer is selected from at least one of polyethylene, polypropylene, and ethylene-propylene copolymer.
17. The encapsulating film for a perovskite solar cell module according to claim 14, characterized in that, The acid neutralizer is selected from at least one of magnesium stearate, zinc stearate, and calcium stearate.
18. The encapsulating film for a perovskite solar cell module according to claim 13 or 14, characterized in that, The silane coupling agent contained in the fourth polymer layer is selected from at least one of mercaptosilane, epoxysilane, aminosilane, methacryloxysilane, vinylsilane, and isocyanate-based silane.
19. The encapsulating film for a perovskite solar cell module according to claim 1, characterized in that, The fifth polymer layer contains an ethylene-vinyl alcohol copolymer and an optional light stabilizer.
20. The encapsulating film for a perovskite solar cell module according to claim 19, characterized in that, Based on the total weight of the fifth polymer layer, the content of the ethylene-vinyl alcohol copolymer is 98.5~99.5 wt%, and the content of the light stabilizer is 0.5~1.5 wt%.
21. The encapsulating film for a perovskite solar cell module according to claim 19, characterized in that, The ethylene-vinyl alcohol copolymer contains 25-45 wt% ethylene structural units and 55-75 wt% vinyl alcohol structural units.
22. The method for preparing the encapsulating film for a perovskite solar cell module according to any one of claims 1 to 21, characterized in that, The method includes mixing the raw materials required for the first polymer layer, the second polymer layer, the third polymer layer, the fourth polymer layer, and the fifth polymer layer evenly and then adding them to an extruder. The extrusion temperature of each layer is set, and the layers are cast through the same die according to the preset thickness of each layer to obtain the encapsulating film for the perovskite solar cell module.
23. The method for preparing the encapsulating film for a perovskite solar cell module according to claim 22, characterized in that, The extrusion temperature of the first polymer layer is 140~180℃; the extrusion temperature of the second polymer layer is 160~180℃; the extrusion temperature of the third polymer layer is 140~160℃; the extrusion temperature of the fourth polymer layer is 80~180℃; and the extrusion temperature of the fifth polymer layer is 160~180℃.
24. The application of the encapsulating film for perovskite solar cell modules according to any one of claims 1 to 21 in perovskite solar cell modules.
Citation Information
Patent Citations
Heterojunction packaging integrated film of dual-protection copper gate and preparation method of heterojunction packaging integrated film
CN115449314A
Thermoplastic grafting and casting integrated POE (Polyolefin Elastomer) adhesive film and preparation method thereof
CN117004352A