A waspaloy nickel-based superalloy and a method of making the same
By adjusting the composition and process of Waspaloy nickel-based superalloys, the precipitation of MC-type carbides was controlled, the problem of η-phase precipitation was solved, the high-temperature creep performance was improved while maintaining room temperature strength, and a cost-effectiveness balance was achieved.
Patent Information
- Application Number
- CN202311543848.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-20
AI Technical Summary
During long-term high-temperature service, existing Waspaloy nickel-based superalloys exhibit a large amount of η-phase (Ni₃Ti) precipitation, which severely impairs the alloy's high-temperature creep performance. Controlling the precipitation and size of MC-type carbides to suppress η-phase precipitation has become crucial.
By adjusting the alloy composition and reducing the Ti content, the precipitation of MC-type carbides is controlled, ensuring that MC-type carbides are almost not precipitated or precipitated in very small amounts, thereby inhibiting the precipitation of η phase, improving high-temperature creep performance, and refining the microstructure through multi-stage forging and heat treatment.
It effectively suppresses the precipitation of the η phase, improves the high-temperature creep performance of Waspaloy nickel-based superalloys, maintains stable room temperature strength, reduces production costs, and has good market application prospects.
Smart Images

Figure CN117701946B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature alloy technology, and particularly relates to a Waspaloy nickel-based high-temperature alloy and its preparation method. Background Technology
[0002] Waspaloy nickel-based superalloys are widely used in high-temperature and high-pressure applications such as aero-engine blades and steam turbine blades, exhibiting high strength and corrosion resistance under high-temperature conditions. A major drawback of Waspaloy alloys is the significant precipitation of the η-phase (Ni3Ti) during long-term high-temperature service, which severely impairs the alloy's high-temperature creep resistance. Recent research has found that preventing the precipitation of MC-type carbides, or ensuring only a very small amount of small-sized MC-type carbides, can significantly reduce or inhibit the precipitation rate of the η-phase. This is because the original alloy has a relatively high Ti content, leading to the formation of a high volume fraction of MC-type carbides, such as... Figure 1 As shown. Therefore, controlling the precipitation and size of MC-type carbides is key to controlling the η phase and thus improving its high-temperature creep performance. Researchers urgently need to provide practical solutions to control the amount of MC-type carbides. Summary of the Invention
[0003] The purpose of this invention is to overcome at least one of the shortcomings of the prior art and provide a Waspaloy nickel-based superalloy and its preparation method. By adjusting the composition, the required Ti element for MC-type carbides is reduced, so that MC-type carbides are hardly precipitated or precipitated in very small amounts, thereby effectively suppressing the precipitation of the harmful η phase, improving the high-temperature creep performance of the Waspaloy nickel-based superalloy, and maintaining stable room temperature strength.
[0004] The technical solution of the present invention is: a Waspaloy nickel-based superalloy, wherein the composition of the Waspaloy nickel-based alloy includes 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.04-0.06 wt% Zr and the balance Ni and unavoidable impurities.
[0005] As a further improvement to this technical solution, the mass fraction of Ti is a wt%, the mass fraction of Al is b wt%, and a and b satisfy the relationship that the sum of a and b is in the range of 3.9-4.1.
[0006] As a further improvement to this technical solution, the volume fraction of MC-type carbides in the Waspaloy nickel-based superalloy is no more than 1%.
[0007] As a further improvement to this technical solution, the composition of the Waspaloy nickel-based alloy includes 1 wt% Ti, 3 wt% Al, 19.5 wt% Cr, 13.5 wt% Co, 4.3 wt% Mo, 0.07 wt% C, 0.05 wt% Zr and the balance Ni and unavoidable impurities.
[0008] This invention also provides a method for preparing Waspaloy nickel-based superalloys, comprising the following steps:
[0009] The raw material preparation steps include preparing 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.04-0.06 wt% Zr and the balance Ni;
[0010] The smelting step involves mixing the prepared raw materials of various elements and placing them in a smelting furnace for smelting.
[0011] As a further improvement to this technical solution, the preparation method further includes a multi-stage forging step, which includes at least a first-stage forging and a second-stage forging.
[0012] As a further improvement to this technical solution, the forging temperature range of the first stage forging is 1000℃-1200℃, and the forging deformation is 35%-45%, to obtain a first forged nickel-based high-temperature alloy; the forging temperature range of the second stage forging is 1000℃-1200℃, and the forging deformation is 55%-65%, to obtain a second forged nickel-based high-temperature alloy.
[0013] As a further improvement to this technical solution, the preparation method also includes a heat treatment step, in which the nickel-based superalloy after multi-stage forging is heat-treated to obtain the final state nickel-based superalloy.
[0014] As a further improvement to this technical solution, the heat treatment step is a multi-stage heat treatment, including at least a first-stage heat treatment, a second-stage heat treatment, and a third-stage heat treatment; the first-stage heat treatment temperature is 1000℃-1100℃, and the heat treatment time is more than 3 hours; the second-stage heat treatment temperature is 800℃-850℃, and the heat treatment time is more than 20 hours; the third-stage heat treatment temperature is 700℃-780℃, and the heat treatment time is more than 15 hours.
[0015] As a further improvement to this technical solution, the multi-stage forging step also includes a solution treatment step between two adjacent forging stages; the solution treatment step includes a first solution treatment step between the first forging step and the second forging step, wherein the first forged nickel-based superalloy is placed at any constant temperature between 1050℃ and 1100℃ for 3-5 hours.
[0016] This invention provides a Waspaloy nickel-based superalloy, the composition of which includes 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.04-0.06 wt% Zr, and the balance Ni and unavoidable impurities. The Waspaloy nickel-based superalloy and its preparation method provided by this invention, through composition adjustment, reduce the Ti element required for MC-type carbide precipitation, thereby ensuring that MC-type carbides precipitate almost none or in very small amounts, effectively suppressing the precipitation of the harmful η-phase, improving the high-temperature creep performance of the Waspaloy nickel-based superalloy, increasing the alloy's strength, and reducing the alloy's production cost, thus showing good market application prospects. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a schematic diagram of η-phase precipitation in the microstructure of existing Waspaloy nickel-based superalloys provided in the background section.
[0019] Figure 2 The provided image shows the microstructure of Waspaloy nickel-based superalloys in the prior art.
[0020] Figure 3 This is a microstructure diagram of the Waspaloy nickel-based superalloy provided in an embodiment of the present invention;
[0021] Figure 4 These are test graphs of the high-temperature creep performance of Waspaloy nickel-based alloy (3Ti1Al) in the prior art and Waspaloy nickel-based alloy (1Ti3Al) in the embodiments of the present invention at 740°C and 310MPa stress.
[0022] Figure 5The diagram shows a comparison of the fracture strength of Waspaloy nickel-based alloy (3Ti1Al) in the prior art and Waspaloy nickel-based alloy (1Ti3Al) in the embodiments of the present invention. Detailed Implementation
[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0024] In the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0025] The various specific technical features and embodiments described in the detailed embodiments can be combined in any suitable manner without contradiction. For example, different implementation methods can be formed by combining different specific technical features / embodiments. In order to avoid unnecessary repetition, the various possible combinations of the various specific technical features / embodiments in this invention will not be described separately.
[0026] This invention provides a Waspaloy nickel-based superalloy, the composition of which includes 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.04-0.06 wt% Zr, and the balance Ni and unavoidable impurities. Compared to the Ti content in traditional Waspaloy nickel-based superalloys (generally greater than 3 wt% to ensure the content of the main strengthening phase γ'-Ni3(Al,Ti), reducing Ti would decrease strength), the Ti content provided in this invention is 0.8-1.2 wt%, a significant reduction. It should be noted that the MC-type carbides in the Waspaloy nickel-based superalloy are mainly Ti-C compounds, and since Ti is the main forming element required for MC-type carbides... The significant reduction in element content greatly reduces the precipitation of MC-type carbides, or in other words, it almost eliminates the precipitation of MC-type carbides (minimum or negligible precipitation), thereby effectively suppressing the precipitation of the harmful η-phase. Specifically, the η-phase is Ni3Ti, requiring 25 at.% Ti. In the absence or minimal precipitation of MC-type carbides, the titanium content is also relatively reduced, resulting in a smaller amount of η-phase (Ni3Ti). Simultaneously, the increased Al content ensures the volume fraction of the main strengthening phase γ'-Ni3(Al,Ti) in the Waspaloy nickel-based superalloy, thus helping to maintain its overall room temperature performance stability. This improves the high-temperature creep performance of the Waspaloy nickel-based superalloy without significantly compromising its strength and toughness at room temperature. Furthermore, by reducing the content of the more expensive Ti element and increasing the content of the less expensive Al element, the overall material cost of the Waspaloy nickel-based superalloy provided in this embodiment is correspondingly reduced, demonstrating good market application prospects.
[0027] In some embodiments, the mass fraction of Ti is awt%, the mass fraction of Al is bwt%, and the relationship between a and b is: the sum of a and b is in the range of 3.9-4.1; in this embodiment, the relationship between a and b is: a+b=4, and the provided Waspaly nickel-based alloy with composition 1Ti3Al and 1.1Ti2.9Al has good overall stability of creep performance at room temperature and high temperature.
[0028] In some embodiments, the Waspaloy nickel-based alloy comprises 1 wt% Ti, 3 wt% Al, 19.5 wt% Cr, 13.5 wt% Co, 4.3 wt% Mo, 0.07 wt% C, 0.05 wt% Zr, and the balance Ni, as well as unavoidable impurities. It is placed in a melting furnace and melted using vacuum induction melting at a temperature between 1700-1900°C to form alloy ingots. Specifically, before vacuum induction melting, the alloy is prepared according to its composition, including Ti rods (TA2), Cr blocks, Co blocks, NiMo alloy, Ni+C mixture, Al blocks (99.99), and Ni blocks. The Ni+C mixture is made by mixing pure Ni powder and pure C powder and sintering them into cubes. During vacuum induction melting, the raw materials are added in the following order: First, three-quarters of the electrolytic Ni cubes are placed at the bottom of the furnace, with a height not exceeding one-third of the crucible depth. Next, approximately two-thirds of the required number of Cr cubes are placed in the middle of the crucible. Then, Co cubes and NiMo alloy are added. The remaining electrolytic Ni cubes are placed at the top of the crucible. Finally, the remaining Cr cubes are placed in the first compartment of the top charging chamber of the induction furnace. After removing the surface layer of the ingot on a lathe, it is manually hot-forged into bars on a 1-ton forging machine. The forging temperature is not lower than 1100℃. If the temperature is too low during hot forging, the ingot is returned to the furnace for continued holding to prevent cracking, resulting in the Waspaloy nickel-based alloy. The microstructure of the Waspaloy nickel-based alloy is shown in the diagram below. Figure 3 As shown; by observing the microstructure of the existing Waspaloy nickel-based alloy (3Ti1Al) (e.g.) Figure 2 As shown), the existing Waspaloy nickel-based alloy (3Ti1Al, specifically composed of 3wt% Ti, 1wt% Al, 19.5wt% Cr, 13.5wt% Co, 4.3wt% Mo, 0.07wt% C, 0.05wt% Zr, and the balance Ni) exhibits a significant amount of harmful η-phase precipitation at grain boundaries, which severely impairs its high-temperature creep performance. In contrast, the Waspaloy nickel-based alloy (1Ti3Al) in this embodiment shows a substantial reduction in the harmful η-phase. Figure 3 As shown; in this embodiment, the volume fraction of MC-type carbides in the Waspaloy nickel-based superalloy is no more than 1%, that is, the amount of MC-type carbides precipitated in the Waspaloy nickel-based superalloy provided in this embodiment is reduced, effectively reducing its proportion in the alloy, and the control effect is significant. The high-temperature creep performance tests of the prior art Waspaloy nickel-based alloy (3Ti1Al) and the Waspaloy nickel-based alloy (1Ti3Al) in this embodiment at 740℃ and 310MPa stress are as follows. Figure 4As shown, the Waspaloy nickel-based alloy (3Ti1Al) requires 200 hours to fracture, while the Waspaloy nickel-based alloy (1Ti3Al) in this embodiment requires 280 hours, effectively improving the creep strength. Through stress fracture testing, its fracture strength is as follows: Figure 5 As shown, tensile strength σ b (ultimate tensile strength), yield strength σ s The yield strength remains essentially unchanged, meaning the room temperature strength remains relatively stable. The elongation (ε) and reduction in area (ψ) of both remain essentially unchanged. Therefore, the Waspaloy nickel-based alloy provided in this embodiment can maintain good toughness. In another embodiment, with 1.1Ti and 2.9Al (other element types and contents remain unchanged), the strength and toughness at room temperature hardly change, maintaining a stable level. Overall performance is stable, and high-temperature creep performance is significantly improved, making it highly practical.
[0029] This invention also provides a method for preparing Waspaloy nickel-based superalloys, comprising a raw material preparation step and a smelting step. The raw material preparation step includes preparing 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.05 wt% Zr, and the balance Ni. The smelting step involves mixing the prepared elemental raw materials (each elemental raw material can be any one or a mixture of pure elemental powder, pure elemental metal blocks, or metal compounds) and smelting them in a smelting furnace. The preparation method further includes a multi-stage forging step, which includes at least a first-stage forging and a second-stage forging.
[0030] In some embodiments, the forging temperature range of the first-stage forging is 1000℃-1200℃, and the forging deformation is 35%-45%, to obtain a first forged nickel-based superalloy; the forging temperature range of the second-stage forging is 1000℃-1200℃, and the forging deformation is 55%-65%, to obtain a second forged nickel-based superalloy.
[0031] In some embodiments, the preparation method further includes a heat treatment step, in which the nickel-based superalloy after multi-stage forging is heat-treated to obtain a final state nickel-based superalloy, which has better stability after forging.
[0032] In some embodiments, the heat treatment step is a multi-stage heat treatment, including at least a first-stage heat treatment, a second-stage heat treatment, and a third-stage heat treatment; the first-stage heat treatment temperature is 1000℃-1100℃, and the heat treatment time is more than 3 hours; the second-stage heat treatment temperature is 800℃-850℃, which is 830℃ in this embodiment, and the heat treatment time is 20 hours; the third-stage heat treatment temperature is 700℃-780℃, which is 750℃ in this embodiment, and the heat treatment time is more than 15 hours. This method effectively refines the MC-type carbide grains, ensuring that the average size of the MC-type carbide is no greater than 1 micrometer, which further helps to reduce the amount of η-phase precipitation.
[0033] In some embodiments, the multi-stage forging step further includes a solution treatment between two adjacent forging stages; the solution treatment includes a first solution treatment between the first forging stage and the second forging stage, wherein the first forged nickel-based superalloy is placed at a constant temperature of 1050℃-1100℃ for 3-5 hours, and in this embodiment it is 1080℃. The solution treatment can effectively homogenize the microstructure, laying a good foundation for the next stage of forging or heat treatment.
[0034] This invention provides a Waspaloy nickel-based superalloy, the composition of which includes 0.8-1.2 wt% Ti, 2.9-3.2 wt% Al, 19-20 wt% Cr, 13-14 wt% Co, 4-4.5 wt% Mo, 0.05-0.1 wt% C, 0.05 wt% Zr, and the balance Ni and unavoidable impurities. The Waspaloy nickel-based superalloy and its preparation method provided by this invention, through composition adjustment, reduce the Ti element required for MC-type carbide precipitation, resulting in almost no or very small precipitation of MC-type carbides, thereby effectively suppressing the precipitation of the harmful η-phase, improving the high-temperature creep performance of the Waspaloy nickel-based superalloy, increasing the alloy's strength, and reducing the alloy's production cost, thus showing good market application prospects.
[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A Waspaloy nickel-based superalloy, characterized in that, The Waspaloy nickel-based superalloy comprises 1 wt% Ti, 3 wt% Al, 19.5 wt% Cr, 13.5 wt% Co, 4.3 wt% Mo, 0.07 wt% C, 0.05 wt% Zr, and the balance Ni, as well as unavoidable impurities; the volume fraction of MC-type carbides in the Waspaloy nickel-based superalloy is not greater than 1%.
2. A method for preparing a Waspaloy nickel-based superalloy, characterized in that, The preparation of the Waspaloy nickel-based superalloy as described in claim 1 includes the following steps: The raw material preparation steps include preparing 1 wt% Ti, 3 wt% Al, 19.5 wt% Cr, 13.5 wt% Co, 4.3 wt% Mo, 0.07 wt% C, 0.05 wt% Zr and the balance Ni; The smelting process involves mixing the prepared raw materials of each element and placing them in a smelting furnace for vacuum induction melting at a temperature between 1700-1900℃. Before vacuum induction melting, the materials are prepared according to the alloy composition, including Ti rods, Cr blocks, Co blocks, NiMo alloy, Ni+C mixture, Al blocks, Ni blocks, and the Ni+C mixture is prepared by uniformly mixing pure Ni powder and pure C powder and sintering it into blocks. During vacuum induction melting, the raw materials are added in the following order: first, three-quarters of the electrolytic Ni blocks are placed at the bottom of the furnace, with the height not exceeding 1 / 3 of the crucible depth; second, 2 / 3 of the required number of Cr blocks are placed in the crucible. In the middle of the crucible, Co blocks and NiMo alloys are placed next, followed by the remaining electrolytic Ni blocks on top of the crucible, and finally the remaining Cr blocks are placed in the first compartment of the top charging chamber of the induction furnace. The preparation method also includes a multi-stage forging step, which includes at least a first-stage forging step and a second-stage forging step. The forging temperature range of the first-stage forging is 1000℃-1200℃, and the forging deformation is 35%-45%, to obtain a first forged nickel-based superalloy. The forging temperature range of the second-stage forging is 1000℃-1200℃, and the forging deformation is 55%-65%, to obtain a second forged nickel-based superalloy. The preparation method further includes a heat treatment step, comprising at least a first-stage heat treatment, a second-stage heat treatment, and a third-stage heat treatment; the first-stage heat treatment temperature is 1000℃-1100℃, and the heat treatment time is more than 3 hours; the second-stage heat treatment temperature is 830℃, and the heat treatment time is 20 hours; the third-stage heat treatment temperature is 750℃, and the heat treatment time is more than 15 hours, so that the average size of the MC-type carbides is no greater than 1 micrometer; the multi-stage forging step further includes a solution treatment between adjacent forging stages; the solution treatment includes a first solution treatment between the first-stage forging and the second-stage forging, wherein the first forged nickel-based superalloy is placed at a solution treatment temperature of 1080℃ for 3-5 hours.
Citation Information
Patent Citations
METHOD FOR MANUFACTURING Ni-BASED HEAT-RESISTANT ALLOY MATERIAL
JP2021080531A
High-temperature sulfidation-corrosion resistant nickel-base alloy
US5900078A