Use of hydroxypropyltrimonium chloride chitosan in the preparation of through-hole electroplating additives
By using hydroxypropyltrimethylammonium chloride chitosan (HACC) as an electroplating leveling agent, the problems of pollution and high cost of existing electroplating additives have been solved, realizing the application of green and environmentally friendly high-performance electroplating additives, improving coating quality and reducing production costs.
Patent Information
- Application Number
- CN202311635043.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-01
AI Technical Summary
Existing electroplating additives pose pollution problems and are costly during the through-hole filling process, making it difficult to achieve the application of green and environmentally friendly high-performance additives.
Hydroxypropyltrimethylammonium chloride chitosan (HACC) was used as an electroplating leveling agent, combined with inhibitors and accelerators, for the preparation of acidic through-hole electroplating solutions. The dosage and process parameters were optimized through electrochemical testing to achieve non-toxic and harmless high-efficiency through-hole filling.
It enables the application of low-cost, environmentally friendly high-performance electroplating additives, reduces the amount of additives used, improves the smoothness and brightness of the coating, and reduces production costs and environmental pollution risks.
Smart Images

Figure CN117702237B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of through-hole electroplating technology and relates to new uses of hydroxypropyltrimethylammonium chloride chitosan. Specifically, it relates to the use of hydroxypropyltrimethylammonium chloride chitosan in the preparation of through-hole electroplating additives, and more specifically to its use as a through-hole electroplating leveling agent and its application in acidic through-hole copper plating. Background Technology
[0002] In the information age, the increasing demand for electronic products has spurred the development of printed circuit boards (PCBs). PCBs are an indispensable component of electronic products, and connecting multilayer PCBs via blind or through-hole vias is one of the most critical technologies. Copper, due to its excellent electrical and thermal conductivity and superior ductility, is ubiquitous in electronic products. Since copper is used to fill through-holes and blind holes, achieving a complete and defect-free copper plating layer within the holes is crucial for ensuring interconnectivity. Currently, the use of electroplating additives is the primary method to guarantee a good plating layer.
[0003] Through-hole copper plating systems are generally high-acid, low-salt systems, and the plating additives are generally divided into three types: inhibitors, accelerators, and leveling agents, as well as chloride ion agents. Through their synergistic effect, the goal is to achieve a bright, smooth, fine-grained plating layer with regular copper crystal orientation. Inhibitors are generally polyethylene glycol (PEG), accelerators are generally sodium polydithiopropane sulfonate (SPS), and chloride ions are generally provided by HCl or NaCl. The generally accepted synergistic mechanism is that PEG is first adsorbed on the surface of the through-hole opening. Copper ions combine with chloride ions and PEG to form a PEG-Cu-Cl-like complex, thus promoting adsorption in the system. The inhibitory effect of PEG is diffusion-controlled, resulting in a long time for PEG to reach the bottom of the through-hole. During this time, SPS carries copper ions to the bottom preferentially, accelerating copper ion deposition. After the bottom is filled, the PEG adsorbed at the opening and corners is gradually replaced by SPS, thereby achieving defect-free filling from the bottom to the opening.
[0004] Current research on leveling agents focuses on organic dye derivatives. Research and use began in the 1980s, revealing that most organic dye electroplating additives possess a large π-conjugated structure, making their electron-conjugated planes more readily adsorbed onto the electrode surface. Currently, many types of organic dyes are used, such as phenazine, DPP, and phenol red dyes, and numerous companies worldwide have conducted extensive research on them. Dye additives can significantly improve the gloss and smoothness of the deposited layer, but they also pose challenges for future wastewater treatment. With increasing national emphasis on environmental protection, high-performance, low-pollution electroplating additives are a new research focus. Furthermore, cost must be considered in the industrial production of electroplating additives, including the production cost of leveling agents, the number of times the electroplating solution can be recycled, the presence of byproducts during electroplating, and the treatment of electroplating wastewater. The most direct production cost issue requires inexpensive and widely available raw materials, an environmentally friendly production process, and high yield. Therefore, designing green, environmentally friendly, low-dosage, and high-performance electroplating leveling agents is a key research focus in this area.
[0005] Chitosan compounds are natural polymers derived from shrimp and crab shells through deacetylation. These compounds are yellowish-white in color, have a structure similar to polysaccharides, and exhibit good biocompatibility, biodegradability, and bioactivity. Hydroxypropyltrimethylammonium chloride chitosan (HACC) has long been industrialized and is inexpensive, non-toxic, and harmless. It has applications in novel bio-encapsulation materials, protein drug carriers, enzyme immobilizers, food preservatives, natural antibacterial agents in wine, and conditioning and moisturizing agents in hair care products. However, its application in the electroplating field has not yet been reported. Summary of the Invention
[0006] This invention addresses the aforementioned problems by exploring the application of hydroxypropyltrimethylammonium chloride chitosan (HACC) in the electroplating field. Electrochemical testing and copper electroplating experiments revealed that HACC requires a lower dosage compared to dye-based leveling agents (DPP quaternary ammonium salt DPP-a), and is also inexpensive, non-toxic, and harmless.
[0007] The structural formulas for HACC and DPP-a are shown below:
[0008]
[0009] In a first aspect, the present invention provides the use of hydroxypropyltrimethylammonium chloride chitosan in the preparation of electroplating additives, and further provides the use of hydroxypropyltrimethylammonium chloride chitosan in the preparation of electroplating leveling agents.
[0010] Preferably, the electroplating leveling agent is a through-hole electroplating leveling agent, and more preferably an acidic through-hole electroplating leveling agent.
[0011] In a second aspect, the present invention provides an additive for filling through-holes in electroplating, comprising hydroxypropyltrimethylammonium chloride chitosan as a leveling agent, wherein the concentration of the hydroxypropyltrimethylammonium chloride chitosan is 0.5 to 3 ppm.
[0012] Preferably, the additives for filling through holes in electroplating provided by the present invention further include 200 ppm of inhibitor and 2 ppm of accelerator, and the inhibitor and accelerator are selected from common substances in the field.
[0013] In a third aspect, the present invention provides a through-hole electroplating solution, comprising 98% H2SO4, CuSO4·5H2O, Cl-, additives, and deionized water, wherein the additives are the additives for electroplating through-holes described in the second aspect above.
[0014] Preferably, the through-hole electroplating solution provided by the present invention is composed of the following components:
[0015]
[0016] The remainder is deionized water.
[0017] A fourth aspect of the present invention provides a method for preparing the above-mentioned through-hole electroplating solution, comprising the following steps: weighing a measured amount of CuSO4·5H2O into a beaker, adding deionized water and stirring to dissolve; then measuring sulfuric acid and slowly adding it to a copper sulfate solution while stirring until the copper sulfate solid is completely dissolved; adding chloride ions, an accelerator, an inhibitor, and a leveling agent to the dissolved copper sulfate solution, and then adding deionized water to the preset capacity, and cooling to room temperature for later use.
[0018] A fifth aspect of the present invention provides a method for through-hole electroplating using the above-described through-hole electroplating solution, comprising the following steps:
[0019] Pour the prepared through-hole electroplating solution into the electroplating tank. Place the pre-treated pre-plating plate directly into the center of the tank as the cathode. After pre-plating for 7 minutes, replace the pre-plating plate with the prepared plate to be plated as the cathode. Use soluble phosphor bronze plates on both sides as anodes. Use a DC power supply and air bubbling to stir the plating solution at a current density of 2A / dm³. 2 Electroplating time: 70 minutes;
[0020] Through-hole electroplating was performed using a soluble phosphor bronze plate as the anode and a PCB board with a through-hole diameter of 0.3 mm as the cathode, employing air agitation at a rate of 2 A / dm². 2 After electroplating at room temperature for 70 minutes at current density, a smooth, bright, and high TP value through-hole filling layer is obtained.
[0021] The pretreatment method for pre-plated plates includes three steps: degreasing, pickling, and water washing, as detailed below:
[0022] Degreasing: Use commercially available degreasing agents to remove oily stains from the surface of the plated sheet for 1.5-2 minutes;
[0023] Pickling: Shake the plated plate in the pickling solution for 1-2 minutes;
[0024] Water washing: Rinse thoroughly with plenty of deionized water to remove any reagent residue from the previous step and ensure that the plated surface is free of other impurities.
[0025] The beneficial protections and effects of this invention are as follows:
[0026] In terms of raw material sources, hydroxypropyltrimethylammonium chloride chitosan (HACC) is a modified product of chitosan. It is highly soluble in water, and HACC has been industrialized, is inexpensive, has good biocompatibility, is environmentally friendly, and conforms to the concept of green chemistry.
[0027] In terms of technical effectiveness, electrochemical testing and copper electroplating revealed that HACC requires a lower dosage compared to dye-based leveling agents (taking DPP quaternary ammonium salt DPP-a as an example). The significance of this invention lies in exploring a high-performance organic electroplating additive that requires less dosage, is readily available, and is environmentally friendly. This invention broadens the application scope of hydroxypropyltrimethylammonium chloride chitosan (HACC). Attached Figure Description
[0028] The present disclosure will be further described below with reference to the accompanying drawings, which are shown only for illustrating the embodiments of the present disclosure and are not intended to limit the scope of the present disclosure.
[0029] Figure 1 The cyclic voltammograms are for HACC and DPP-a at the same concentration.
[0030] Figure 2 The graph shows the polarization curves of HACC and DPP-a at the same concentration.
[0031] Figure 3 Add a graph to the galvanostatic timing of the HACC molecule.
[0032] Figure 4 Add a graph to the galvanostatic timing of the DPP-a molecule.
[0033] Figure 5 Metallographic image of electroplated through-holes for HACC molecules as a leveling agent. Detailed Implementation
[0034] The following embodiments and experimental examples further illustrate the present invention and should not be construed as limiting the invention. The embodiments do not include a detailed description of conventional methods, which are well known to those skilled in the art and described in numerous publications.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as are familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention, and the preferred embodiments and materials described in the Detailed Description section are for illustrative purposes only.
[0036] I. Reagents and Materials
[0037] The pharmaceuticals used in the embodiments of this invention are shown in Table 1 below:
[0038] Table 1 Summary of drugs used in the examples
[0039]
[0040] The present invention will be further illustrated below through examples, with the aim of better understanding the content of the present invention. The examples given do not limit the scope of protection of the present invention.
[0041] Example 1 Cyclic Voltammetry Test of Compound HACC
[0042] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Under the condition of rotating at 2000 rpm, 1 mL of a 1 mg / L HACC aqueous solution was added dropwise to 100 mL of the copper sulfate solution, and its cyclic voltammetry curve was tested.
[0043] Cyclic voltammetry of compound DPP-a in Comparative Example 1
[0044] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Under the condition of rotating at 2000 rpm, 1 mL of a 1 mg / L compound DPP-a solution was added dropwise to 100 mL of the copper sulfate solution, and its cyclic voltammetry curve was tested.
[0045] Figure 1 The comparison of cyclic voltammetry results for HACC and DPP-a is shown, indicating that the oxidation peak height of the blank curve is 36.65 A / dm. 2 The addition of HACC and DPP-a reduced the maximum peak height and peak area, indicating that the two compounds can inhibit copper ion deposition. The maximum peak height of HACC was 17.28 A / dm². 2 The decrease was 19.37 A / dm. 2The maximum peak height of DPP-a is 26.74 A / dm. 2 The decrease was 9.91A / dm. 2 The inhibitory effect of HACC is 1.9 times that of DPP-a, indicating that HACC requires a smaller dosage than DPP-a to achieve the same inhibitory effect.
[0046] Example 2: Polarization curve test of compound HACC
[0047] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Under the condition that the three-electrode system rotated at 2000 rpm, 1 mL of 1 mg / L HACC solution was added dropwise to 100 mL of the copper sulfate solution, and its polarization curve was tested.
[0048] Polarization curve test of compound DPP-a in Comparative Example 2
[0049] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Under the condition that the three-electrode system rotated at 2000 rpm, 1 mL of DPP-a solution with a concentration of 1 mg / L was added dropwise to 100 mL of the copper sulfate solution, and its polarization curve was tested.
[0050] Figure 2 The polarization curves of compounds HACC and DPP-a at the same concentration in the base plating solution are shown. The graph shows that when only the base plating solution is present, the current density begins to increase from around 0V, indicating that copper ions begin to deposit at 0V. The smaller the inflection point voltage of the curve, the greater the polarization potential of the compound. The addition of compounds HACC and DPP-a results in larger polarization potentials; HACC's polarization potential reaches -0.17V, and DPP-a's is -0.12V. A larger absolute value of the polarization potential indicates a stronger ability of the compound to inhibit copper plating. Therefore, at the same concentration, HACC's inhibition ability is stronger than DPP-a, consistent with previous cyclic voltammetry results.
[0051] Example 3: Current-Gaussian Timing Curve Test of Compound HACC
[0052] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Two rotation speeds were used in the three-electrode system: a high speed of 1500 rpm and a low speed of 150 rpm. The change in electrode potential in the base electroplating solution with the addition of electroplating additives was measured under constant current. The total test duration was 4000 seconds. At 1000 seconds, 2000 seconds, and 3000 seconds, 200 ppm of polyethylene glycol (PEG) (average molecular weight 10000), 2 ppm of sodium polydisulfide dipropane sulfonate (SPS), and 0.2 ml of a 1 mg / L HACC solution were added to the solution.
[0053] Comparative Example 3: galvanostatic timing addition curve test of compound DPP-a
[0054] A copper sulfate solution containing 60 g / L CuSO4·5H2O, 140 μL HCl, and 180 g / L H2SO4 was prepared. A Pt rotating disk electrode was used as the working electrode, a platinum wire electrode as the counter electrode, and Ag / AgCl as the reference electrode. Two rotation speeds were used in the three-electrode system: a high speed of 1500 rpm and a low speed of 150 rpm. The change in electrode potential in the base electroplating solution with the addition of electroplating additives was measured under constant current. The total test duration was 4000 seconds. At 1000 seconds, 2000 seconds, and 3000 seconds, 200 ppm of polyethylene glycol (PEG) (average molecular weight 10000), 2 ppm of sodium polydisulfide dipropane sulfonate (SPS), and 0.2 ml of a 1 mg / L LPP-a solution were added to the solution.
[0055] Previous electrochemical tests revealed that the compound HACC possesses strong copper plating inhibition capabilities, and this was further investigated using a galvanostatic timing test. For example... Figure 3 and Figure 4As shown, when the inhibitor PEG 10000 and the accelerator SPS were added at 1000 seconds and 2000 seconds respectively, the potential change trend generally showed a decrease followed by an increase, consistent with the effects of the two compounds. The addition of compound HACC suppressed the depolarization of SPS in the electroplating solution, causing the potential to shift negatively. This is due to the synergistic effect of compound HACC with PEG and SPS; the addition of compound HACC further enhanced the inhibition of copper deposition. The convection at the orifice and inner wall of the hole during actual through-hole copper plating was simulated using high rotation speeds of 1500 rpm and low rotation speeds of 150 rpm. The potential difference at different rotation speeds was defined as Δη = η(150 rpm) - η(1000 rpm). After the addition of compound HACC, Δη ≈ 13 mV, a positive value, indicating that the adsorption behavior of compound HACC is convection-dependent adsorption; it is more easily adsorbed in areas of strong convection, thus achieving the effect of inhibiting copper deposition on the hole surface compared to the inside of the hole. Similarly, DPP-a also showed the same trend Δη≈7mV, which indicates that the convective adsorption of DPP-a is weaker than that of HACC.
[0056] The performance comparison data of leveling agents HACC and DPP-a are summarized in Table 2, as follows:
[0057] Table 2 Comparison of electrochemical performance data between HACC and DPP-a
[0058] Serial Number compound Cyclic Volt-Ampere Decrease Inflection point value of polarization curve Timing Add Curve Δη 1 HACC 19.37 -0.17V 13mV 2 DPP-a 9.91 -0.12V 7mV
[0059] Table 2 shows a comparison of the electrochemical performance of HACC and DPP-a. It can be seen that at the same concentration, HACC exhibits better performance than DPP-a, indicating that in practical applications, the amount of HACC used as an additive is less than that of DPP-a, which would bring considerable benefits in industrial production. Furthermore, HACC is green, pollution-free, and harmless to the environment and human body, and can be purchased directly. DPP-a, on the other hand, requires organic synthesis, which is cumbersome, difficult, and costly, and is harmful to the environment and human health. Actual through-hole filling experiments have demonstrated that HACC, as a leveling agent, can meet the requirements for efficient through-hole filling. Therefore, HACC outperforms pigment-based leveling agents and has commercial potential.
[0060] Application Example 1: Through-hole electroplating solution and electroplating
[0061] 1. Plating solution formulation:
[0062]
[0063] 2. Through-hole electroplating
[0064] The specific steps are as follows:
[0065] (1) Preparation of electroplating solution
[0066] Weigh a measured amount of copper sulfate pentahydrate into a beaker, add deionized water and stir to dissolve; measure sulfuric acid and slowly add it to the copper sulfate solution while stirring until the copper sulfate solid is completely dissolved; add chloride ions, accelerator, inhibitor and leveling agent to the dissolved copper sulfate solution, and add deionized water to the mark; cool to room temperature and use.
[0067] (2) Pretreatment of plated sheet: degreasing - pickling - water washing
[0068] Degreasing: During the preparation process, the surface of the plate to be plated may be contaminated with oil, stains, etc. In order to remove the influence of oily impurities, it is necessary to use a commercially available degreasing agent to remove the oily stains on the surface of the plate to be plated for 1.5-2 minutes.
[0069] Pickling: The purpose of pickling is to remove the residue of the degreasing agent in the previous step, and at the same time remove the oxide layer on the copper surface to ensure that no oxides participate in the reaction and consume electrons during the subsequent electroplating process. The plate to be plated is shaken in the pickling agent for 1-2 minutes.
[0070] Water washing: Rinse thoroughly with plenty of deionized water to remove any reagent residue from the previous step and ensure that the plated surface is free of other impurities.
[0071] (3) Through-hole electroplating
[0072] Pour the prepared electroplating solution into a 1.5L Haring tank. Place the pre-treated plate directly into the center of the Haring tank as the cathode. After pre-plating for 7 minutes, replace the pre-plated plate with the prepared plate to be plated as the cathode. Use soluble phosphor bronze plates as anodes on both sides. Use a DC power supply and air bubbling to stir the plating solution at a current density of 2A / dm³. 2 Electroplating time: 70 minutes.
[0073] A Harlem trough through-hole electroplating experiment was conducted using a soluble phosphor bronze plate as the anode and a PCB board with a through-hole diameter of 0.3 mm as the cathode. Air agitation was employed at a rate of 2 A / dm³. 2 After electroplating at room temperature for 70 minutes at current density, a smooth, bright, and high TP value through-hole filling layer was obtained. Figure 5 ).
[0074] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited to the embodiments described. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of the present invention, and these equivalent modifications or substitutions are all included within the scope defined by the claims of this application.
Claims
1. The application of an additive in electroplating through-hole filling, characterized in that, The additives include hydroxypropyltrimethylammonium chloride chitosan as a leveling agent, with a concentration of 0.5~3ppm. The electroplating filling of the through holes is a through-hole electroplating copper system.
2. The application of the additive according to claim 1 in electroplating through-hole filling, characterized in that, The additives also include 200 ppm of inhibitor and 2 ppm of accelerator.
3. A through-hole electroplating solution, characterized in that, Composed of 98% H2SO4, CuSO4·5H2O, Cl - It consists of additives and deionized water, wherein the additives are those described in claim 2.
4. The through-hole electroplating solution according to claim 3, characterized in that, It consists of the following components: H2SO4 180g / L CuSO4·5H2O 60g / L Cl - 140uL / L Inhibitor 200ppm Accelerator 2ppm Leveling agent HACC 2ppm The remainder is deionized water.
5. The method for preparing the through-hole electroplating solution according to claim 3 or 4, characterized in that, Includes the following steps: Weigh a measured amount of CuSO4·5H2O into a beaker, add deionized water and stir to dissolve; then measure sulfuric acid and slowly add it to the copper sulfate solution while stirring until the copper sulfate solid is completely dissolved; add chloride ions, accelerator, inhibitor and leveling agent to the dissolved copper sulfate solution respectively, then add deionized water to the preset capacity, and cool to room temperature for later use.
6. A method for through-hole copper plating using the through-hole plating solution according to claim 3 or 4, characterized in that, Includes the following steps: Pour the prepared through-hole electroplating solution into the electroplating tank. Place the pre-treated pre-plating plate directly into the center of the tank as the cathode. After pre-plating for 7 minutes, replace the pre-plating plate with the prepared plate to be plated as the cathode. Use soluble phosphor bronze plates on both sides as anodes. Use a DC power supply and air bubbling to stir the plating solution at a current density of 2A / dm³. 2 Electroplating time: 70 minutes; Through-hole electroplating was performed using a soluble phosphor bronze plate as the anode and a PCB board with a through-hole diameter of 0.3 mm as the cathode, employing air agitation at a rate of 2 A / dm². 2 After electroplating at room temperature for 70 minutes at current density, a smooth, bright, and high TP value through-hole filling layer is obtained.
7. The method for through-hole copper plating according to claim 6, characterized in that: in, The pretreatment method for pre-plated plates includes three steps: degreasing, pickling, and water washing, as detailed below: Degreasing: Use commercially available degreasing agents to remove oily stains from the surface of the plated sheet for 1.5-2 minutes; Pickling: Shake the plated plate in the pickling solution for 1-2 minutes; Water washing: Rinse thoroughly with plenty of deionized water to remove any reagent residue from the previous step and ensure that the plated surface is free of other impurities.
Citation Information
Patent Citations
Quaternary ammonium salt leveling agent, preparation method thereof, electroplating liquid containing quaternary ammonium salt leveling agent and electroplating method
CN114031769A