A method for preparing zinc concentrate by using zinc-containing blast furnace dust
By using methods such as crushing and dispersing slurry preparation, flotation agent separation, and airflow pulverization and classification, the problem of substandard zinc recovery from blast furnace dust was solved, resulting in high-grade zinc concentrate and achieving environmentally friendly and efficient resource utilization.
Patent Information
- Application Number
- CN202311455777.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-03
AI Technical Summary
Existing technologies are insufficient to effectively recover zinc from blast furnace dust, resulting in substandard zinc grades and inefficient and environmentally unfriendly processing methods.
The method of separating iron, zinc and carbon by crushing, dispersing and adjusting the slurry, and using flotation agents, combined with air jet milling and particle size classification, separates and enriches zinc concentrate. Sodium alkylbenzene sulfonate and kerosene are used as flotation agents, and particle size classification is carried out by hydrocyclones or air jet classifiers.
It achieves efficient enrichment of zinc concentrate, is simple to operate, low in cost, meets environmental protection requirements, and is easy to apply industrially.
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary resource comprehensive recycling of blast furnace dust, specifically to a method for preparing zinc concentrate using zinc-containing blast furnace dust. Background Technology
[0002] Blast furnace dust is a byproduct of blast furnace ironmaking. It consists of coarse particles carried out with blast furnace gas and obtained through gravity dust removal, followed by fine particles obtained through bag filter dust removal. Blast furnace dust mainly contains iron, carbon, and zinc. Current disposal methods include stockpiling or landfilling, incorporation into sintering processes, use as an ingredient in cement and other building materials, and comprehensive recycling. Comprehensive recycling methods primarily involve mineral processing, pyrometallurgical processes, hydrometallurgical processes, or a combination of two or three of these methods, mainly involving the recovery of iron, carbon, and zinc.
[0003] Chinese patent CN110743714B discloses a method for enriching and recovering zinc from blast furnace gas mud. The method uses flotation to remove zinc. The original gas mud has a zinc grade of 10.50%. After flotation, the zinc grade of the zinc-rich material is 21.58%. The zinc content of this zinc-rich material is not high and cannot meet the standard for zinc concentrate. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing zinc concentrate using zinc-containing blast furnace dust. This method is easy to operate, has a good zinc enrichment effect, is green and environmentally friendly, and is easy to industrialize. It can turn waste into treasure and obtain zinc concentrate with high economic value.
[0005] To achieve the above-mentioned objectives, this invention provides a method for preparing zinc concentrate using zinc-containing blast furnace dust, comprising the following steps:
[0006] Step (1): After mixing zinc-containing blast furnace dust and water, the mixture is crushed, dispersed, and slurry-prepared to obtain a slurry.
[0007] Step (2): Add the first flotation agent to the slurry for flotation to separate the iron and zinc in the slurry, and obtain iron-poor zinc-rich slurry and iron-rich zinc-poor slurry respectively; wherein, the first flotation agent is sodium alkylbenzene sulfonate;
[0008] Step (3): Add a second flotation agent to the iron-rich and zinc-rich material slurry to remove carbon-containing particles from the iron-rich and zinc-rich material slurry by flotation, and obtain carbon-rich and zinc-rich material slurry and carbon-rich and zinc-rich material slurry. Filter the carbon-rich and zinc-rich material slurry to obtain zinc-rich material; wherein, the second flotation agent is a compound of sodium dodecylbenzene sulfonate and kerosene or No. 260 aviation kerosene;
[0009] Step (4): The zinc-rich material is successively subjected to preliminary crushing, drying, sieving, and air-jet crushing of the undersize material before being transported to a hydrocyclone or air-jet classifier for particle size classification to obtain iron-rich and zinc-poor material and zinc concentrate.
[0010] Typically, zinc-containing blast furnace dust refers to blast furnace gravity ash, blast furnace gas ash, blast furnace bag filter ash, TRT ash, or blast furnace gas sludge carried out with blast furnace gas during the blast furnace ironmaking process. The zinc content of blast furnace gravity ash or blast furnace gas ash is usually around 0.1% to 1.5%, while the zinc content of blast furnace bag filter ash, TRT ash, or blast furnace gas sludge is between 0.1% and 25%. The zinc content of the raw materials required for the method in this application must be ≥0.5%. Due to environmental protection requirements, except for blast furnace dust transported by tank truck which does not require water spraying for dust removal... For other transportation methods, the blast furnace dust is usually sprayed with water to prevent dust from being generated during the ash discharge process. Since the temperature of the blast furnace dust is usually about 200°C and it contains soluble salts, the blast furnace dust will clump after being sprayed with water. Clumping will cause the overall particle size distribution to change. Therefore, for zinc-containing blast furnace dust that has clumping, water is added and ball milling is used to disperse it. This restores the original particle size distribution as much as possible without changing it or with minimal change, so as to facilitate subsequent processing.
[0011] In one specific embodiment of the present invention, when adding the first flotation agent, the material should be added while stirring and aerating to enhance the foaming effect. Simultaneously, the generated foam should be scraped off using a flotation machine until almost no foam is produced. The resulting foam is a lean iron and rich zinc slurry, and the remaining tailings are a rich iron and lean zinc slurry. The rich iron and lean zinc slurry obtained after filtration can be recycled as an iron-containing raw material. The filtrate is returned to the ball mill for dispersing and slurry preparation process, while the lean iron and rich zinc slurry proceeds to the next step of flotation decarbonization.
[0012] In another specific embodiment of the present invention, when adding the second flotation agent, the material should be added while stirring and aerating to enhance the foaming effect. Simultaneously, the generated foam should be scraped off using a flotation machine until almost no foam is produced. The obtained foam is a carbon-rich, zinc-poor slurry, and the remaining tailings are a carbon-poor, zinc-rich slurry. The former is filtered to obtain filtrate and carbon-rich, zinc-poor material that can be recycled as carbon raw material. The filtrate is returned to the ball milling and dispersing process.
[0013] According to the present invention, a method for preparing zinc concentrate using zinc-containing blast furnace dust is preferably described in step (1), wherein the mass ratio of zinc-containing blast furnace dust to water is 2-5:1.
[0014] According to the present invention, a method for preparing zinc concentrate using zinc-containing blast furnace dust is preferably described in step (1), where the equipment used in the crushing, dispersing and slurry preparation step is a ball mill, a vertical mill, or a pulverizer, and the grinding balls can be made of steel balls, zirconium oxide, or silicon oxide.
[0015] According to the present invention, in a method for preparing zinc concentrate using zinc-containing blast furnace dust, preferably, in step (1), the mass ratio of grinding balls to dry zinc-containing blast furnace dust is 6-12:1.
[0016] In this invention, grinding balls with a diameter of 20 mm account for 5% to 15% of the total mass of the grinding balls, grinding balls with a diameter of 15 mm account for 25% to 35% of the total mass of the grinding balls, grinding balls with a diameter of 10 mm account for 25% to 35% of the total mass of the grinding balls, and grinding balls with a diameter of 5 mm account for 25% to 35% of the total mass of the grinding balls; preferably, the ball milling or vertical milling time is 5-10 minutes, and the motor frequency is 10-30 Hz.
[0017] According to the present invention, a method for preparing zinc concentrate using zinc-containing blast furnace dust is preferably described in step (1), where the solid content of the slurry after preparation is 16wt% to 30wt%.
[0018] According to the present invention, in a method for preparing zinc concentrate using zinc-containing blast furnace dust, preferably, in step (2), the ratio of the first flotation agent to the dry blast furnace dust is 2-10g:1000g, and the addition rate of the first flotation agent is 1-2g / min.
[0019] According to the present invention, in a method for preparing zinc concentrate using zinc-containing blast furnace dust, preferably, in step (3), the mass percentage of kerosene or No. 260 aviation kerosene in the second flotation agent is 90%-99%, and the mass percentage of sodium dodecylbenzenesulfonate is 1%-10%.
[0020] According to the present invention, in a method for preparing zinc concentrate using zinc-containing blast furnace dust, preferably, in step (3), the ratio of the amount of the second flotation agent to the dry material rich in zinc and low in iron is 100-200g:1000g, and the addition rate of the second flotation agent is 5-20g / min.
[0021] According to the method for preparing zinc concentrate using zinc-containing blast furnace dust according to the present invention, preferably, in step (4), the particle size classification device can be a hydrocyclone or an air classifier, and the classification particle size is 13μm. Particles ≥13μm and <13μm are separated by particle size classification to obtain iron-rich and zinc-poor feedstock and artificial zinc concentrate, respectively.
[0022] According to the present invention, a method for preparing zinc concentrate using zinc-containing blast furnace dust is preferably described in step (4), whereby the zinc-rich material is sequentially subjected to preliminary crushing, drying, sieving, and air-jet crushing of the undersize material before being transported to a hydrocyclone or air-jet classifier for particle size classification, wherein the diameter of the undersize material is not greater than 2 mm.
[0023] According to the method for preparing zinc concentrate using zinc-containing blast furnace dust according to the present invention, preferably, in step (4), when the air classifier is an air classifier, the frequency of the air classifier host is 30-80Hz, the frequency of the fan is 40-60Hz, and the air volume is 25-45m³. 3 / min.
[0024] According to the present invention, a method for preparing zinc concentrate using zinc-containing blast furnace dust is preferably described in step (4), when the air classifier is a hydrocyclone, the diameter of the hydrocyclone barrel is 25-150mm, the feed pressure is 0.04-0.1MPa, and the diameter of the hydrocyclone underflow outlet is not less than 6mm.
[0025] As a specific embodiment of the present invention, the diameter of the hydrocyclone barrel is 50-100mm; more preferably, the diameter of the hydrocyclone underflow outlet is 6-24mm.
[0026] The beneficial effects of this invention are:
[0027] The present invention discloses a method for preparing zinc concentrate using zinc-containing blast furnace dust. The method involves using a first flotation agent to separate zinc- and iron-containing minerals in the slurry, then using a second flotation agent to decarbonize the obtained iron-poor and zinc-rich slurry, and then using air jet milling and classification to further separate the zinc- and iron-containing minerals in the carbon-poor and zinc-rich slurry, thereby obtaining high-grade zinc concentrate.
[0028] This method is easy to operate, has a simple process flow, low production cost, good zinc enrichment effect, is green and environmentally friendly, and is easy to industrialize, and can obtain zinc concentrate with high economic value. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples.
[0030] It should be noted that all uses of "first" and "second" in the embodiments of the present invention are for the purpose of distinguishing two entities or parameters with the same name but different names. It is clear that "first" and "second" are only for the convenience of expression and should not be construed as limiting the embodiments of the present invention. Subsequent embodiments will not explain this in detail.
[0031] Example 1
[0032] Example 1 provides a method for preparing zinc concentrate using zinc-containing blast furnace dust, the steps of which include:
[0033] Step (1): After mixing zinc-containing blast furnace dust with a zinc content of 3wt% with water, the mixture is crushed, dispersed and slurry-prepared to obtain a slurry. The mass ratio of zinc-containing blast furnace dust to water is 1:4. When a ball mill is used for the crushing step, the mass ratio of stainless steel grinding balls to dry zinc-containing blast furnace dust is 10:1. Grinding balls with a diameter of 20mm account for 15% of the total mass of grinding balls, grinding balls with a diameter of 15mm account for 25% of the total mass of grinding balls, grinding balls with a diameter of 10mm account for 30% of the total mass of grinding balls, and grinding balls with a diameter of 5mm account for 30% of the total mass of grinding balls. The ball milling time is 10min, the motor frequency is 30Hz, and the solid content of the slurry after preparation is 25wt%.
[0034] Step (2): Add sodium alkylbenzene sulfonate to the slurry for flotation to separate the iron and zinc in the slurry, and obtain iron-poor zinc-rich slurry and iron-rich zinc-poor slurry respectively; the ratio of sodium alkylbenzene sulfonate to dry blast furnace dust is 5g:1000g, and the addition rate of sodium alkylbenzene sulfonate is 2g / min.
[0035] Step (3): Add kerosene and sodium dodecylbenzene sulfonate compound to the iron-rich and zinc-poor material slurry, remove carbon particles from the iron-rich and zinc-poor material slurry by flotation, and obtain carbon-rich and zinc-poor material slurry and carbon-rich and zinc-poor material slurry. Filter the carbon-rich and zinc-poor material slurry to obtain zinc-poor material. The mass ratio of kerosene in the compound is 95wt%, the ratio of the compound to the dry iron-rich and zinc-poor material is 100g:1000g, and the addition rate is 15g / min.
[0036] Step (4): After preliminary crushing and drying, the zinc-rich material is passed through a 2mm mesh screen. The undersize material is then dispersed by air jet milling and conveyed to a hydrocyclone for air jet classification to obtain iron-rich and zinc-poor material and zinc concentrate. The air jet mill is used for dispersion treatment, with an air flow rate of 0.6m³ / min. 3 / min, air pressure is 2Mpa, hydrocyclone barrel diameter is 60mm, feed pressure is 0.08MPa, hydrocyclone underflow diameter is 12mm, classification particle size is 13μm, particles with a particle size not less than 13μm are iron-rich and zinc-poor slurry, particles with a particle size less than 13μm are zinc concentrate.
[0037] The zinc concentrate obtained in Example 1 was found to have a grade of 51.5 wt%.
[0038] Example 2
[0039] Example 2 provides a method for preparing zinc concentrate using zinc-containing blast furnace dust, the steps of which include:
[0040] Step (1): After mixing zinc-containing blast furnace dust with a zinc content of 10wt% with water, the mixture is crushed, dispersed and slurry-prepared to obtain a slurry. The mass ratio of zinc-containing blast furnace dust to water is 1:4. When a ball mill is used for the crushing step, the mass ratio of stainless steel grinding balls to dry zinc-containing blast furnace dust is 10:1. Grinding balls with a diameter of 20mm account for 15% of the total mass of grinding balls, grinding balls with a diameter of 15mm account for 25% of the total mass of grinding balls, grinding balls with a diameter of 10mm account for 30% of the total mass of grinding balls, and grinding balls with a diameter of 5mm account for 30% of the total mass of grinding balls. The ball milling time is 10min, the motor frequency is 30Hz, and the solid content of the slurry after preparation is 25wt%.
[0041] Step (2): Add sodium alkylbenzene sulfonate to the slurry for flotation to separate the iron and zinc in the slurry, and obtain iron-poor zinc-rich slurry and iron-rich zinc-poor slurry respectively; the ratio of sodium alkylbenzene sulfonate to dry blast furnace dust is 5g:1000g, and the addition rate of sodium alkylbenzene sulfonate is 2g / min.
[0042] Step (3): Add kerosene and sodium dodecylbenzene sulfonate compound to the iron-rich and zinc-poor material slurry, remove carbon particles from the iron-rich and zinc-poor material slurry by flotation, and obtain carbon-rich and zinc-poor material slurry and carbon-rich and zinc-poor material slurry. Filter the carbon-rich and zinc-poor material slurry to obtain zinc-poor material. The mass ratio of kerosene in the compound is 95wt%, the ratio of the compound to the dry iron-rich and zinc-poor material is 100g:1000g, and the addition rate is 15g / min.
[0043] Step (4): After preliminary crushing and drying, the zinc-rich material is passed through a 2mm mesh screen. The undersize material is then dispersed by airflow pulverization and conveyed to an airflow classifier for airflow classification to obtain iron-rich, zinc-poor material and zinc concentrate. The main unit frequency of the airflow classifier is 65Hz, the fan frequency is 50Hz, and the airflow volume is 33m³ / h. 3 / min, the grading particle size is 13μm. Particles with a particle size of not less than 13μm are iron-rich and zinc-poor slurry, while particles with a particle size of less than 13μm are zinc concentrate.
[0044] The zinc concentrate obtained in Example 2 was found to have a grade of 56.4 wt%.
[0045] Comparative Example 1
[0046] Comparative Example 1: Zinc-containing blast furnace dust with a zinc content of 10 wt% was treated according to the method of Example 1 of Chinese Patent CN110743714B. The grade of the zinc-rich material was 21.58%, which did not meet the standard of zinc concentrate.
[0047] It should be noted that the components or steps in the above embodiments can be interchanged, substituted, added, or deleted. Therefore, the combinations formed by these reasonable permutations and transformations should also fall within the protection scope of this invention, and the protection scope of this invention should not be limited to the above embodiments.
[0048] The above are exemplary embodiments disclosed in this invention. The order of the disclosed embodiments is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. However, it should be noted that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of this invention (including the claims) is limited to these examples. Various changes and modifications can be made without departing from the scope defined by the claims. The functions, steps, and / or actions of the methods according to the disclosed embodiments described herein do not need to be performed in any particular order. Furthermore, although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular.
[0049] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A method for preparing zinc concentrate using zinc-containing blast furnace dust, characterized in that, Includes the following steps: Step (1): After mixing zinc-containing blast furnace dust and water, the mixture is crushed, dispersed, and slurry-prepared to obtain a slurry. Step (2): Add the first flotation agent to the slurry for flotation to separate the iron and zinc in the slurry, and obtain iron-poor zinc-rich slurry and iron-rich zinc-poor slurry respectively; wherein, the first flotation agent is sodium alkylbenzene sulfonate; Step (3): Add a second flotation agent to the iron-rich and zinc-rich material slurry to remove carbon-containing particles from the iron-rich and zinc-rich material slurry by flotation, and obtain carbon-rich and zinc-rich material slurry and carbon-rich and zinc-rich material slurry. Filter the carbon-rich and zinc-rich material slurry to obtain zinc-rich material; wherein, the second flotation agent is a compound of sodium dodecylbenzene sulfonate and kerosene. Step (4): The zinc-rich material is subjected to preliminary crushing, drying and sieving in sequence. The diameter of the material under the screen is no more than 2 mm. The material under the screen is then air-jet crushed and dispersed and transported to a hydrocyclone or air classifier for particle size classification to obtain iron-rich and zinc-poor material and zinc concentrate. The particle size of the particle size classification device is 13 µm.
2. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (1), the mass ratio of zinc-containing blast furnace dust to water is 2-5:
1.
3. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (1), the equipment used in the crushing and slurry preparation step is a ball mill, a vertical mill, or a pulverizer, and the grinding balls are made of steel balls, zirconium oxide, or silicon oxide.
4. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 3, characterized in that, In step (1), the mass ratio of grinding balls to zinc-containing blast furnace dust dry material is 6-12:
1.
5. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (1), the solid content of the slurry after conditioning is 16wt%~30wt%.
6. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (2), the ratio of the first flotation agent to the dry blast furnace dust is 2-10g:1000g, and the addition rate of the first flotation agent is 1-2g / min.
7. The method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (3), the mass percentage of kerosene in the second flotation agent is 90%-99%, and the mass percentage of sodium dodecylbenzenesulfonate is 1%-10%.
8. A method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 7, characterized in that, In step (3), the ratio of the amount of the second flotation agent to the dry material rich in zinc and low in iron is 100-200g:1000g, and the addition rate of the second flotation agent is 5-20g / min.
9. A method for preparing zinc concentrate using zinc-containing blast furnace dust according to claim 1, characterized in that, In step (4), when the airflow classification device is an airflow classifier, the frequency of the airflow classification host is 30~80Hz, the frequency of the fan is 40~60Hz, and the air volume is 25~45m³ / h. 3 / min; When the air classifier is a hydrocyclone, the diameter of the hydrocyclone barrel is 25-150mm, the feed pressure is 0.04-0.1MPa, and the diameter of the hydrocyclone underflow outlet is not less than 6mm.
Citation Information
Patent Citations
Methods for enriching and recovering zinc from blast furnace gas sludge
CN110743714B
Method for recycling valuable elements from blast furnace gas mud
CN102747228A
Method for recovering zinc, indium and lead in blast furnace cloth bag ash
CN113061734A
Blast furnace cloth bag dedusting ash waste-free treatment method
CN114918038A