A kind of hard ceramic particle and multiple metal powder in-situ generation superhard reinforced phase based on middle-entropy alloy coating and its preparation method

By using composite powder plasma cladding technology of hard ceramic particles and various metal powders, a medium-entropy alloy coating with an ultra-hard reinforcing phase is generated, which solves the problem of insufficient bonding between the matrix phase and the hard phase, achieves high corrosion resistance and wear resistance of the coating, and extends its service life.

CN117721457BActive Publication Date: 2026-11-20HEBEI HANFENG POWER GENERATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311639300.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2026-11-20
Estimated Expiration
2043-12-01

AI Technical Summary

Technical Problem

Existing plasma cladding technology has problems such as insufficient bonding between the matrix phase and hard material and microcracks when preparing medium-entropy/high-entropy alloy coatings. In addition, the medium-entropy/high-entropy alloy powder decomposes and dilutes during the cladding process, resulting in a decrease in the content of medium-entropy/high-entropy phases inside the coating, which affects the corrosion resistance.

Method used

A composite powder of hard ceramic particles and various metal powders is used to generate a medium-entropy alloy coating with an ultra-hard reinforcing phase through plasma cladding. Some of the ceramic powder is completely or partially melted and decomposed to react with the metal powder to generate a medium-entropy alloy phase. The unmelted ceramic particles are dispersed in the coating as a hard phase, achieving metallurgical bonding.

Benefits of technology

It significantly improves the corrosion resistance and wear resistance of the coating, extends its service life, and achieves a coating hardness of over 400HV0.3, with wear resistance significantly superior to traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117721457B_ABST
    Figure CN117721457B_ABST
Patent Text Reader

Abstract

The application discloses a kind of based on hard ceramic particles and a variety of metal powder in-situ generation superhard reinforcing phase's quasi-entropy alloy coating and preparation method thereof, preparation method includes: using plasma cladding method to prepare composite powder into cladding layer;Composite powder uses the mixed powder of metal powder and ceramic powder;When using plasma cladding method to prepare composite powder into cladding layer, a part of ceramic powder completely melts and decomposes, another part of ceramic powder partially melts and decomposes and / or does not melt and decompose, and the ceramic powder that melts and decomposes and metal powder generate quasi-entropy alloy phase, greatly improve corrosion resistance on the basis of original metal;Partially melted and / or unmelted particles are distributed in matrix phase, improve wear resistance.Therefore, the quasi-entropy alloy coating prepared by the preparation method of the application can greatly improve wear resistance and corrosion resistance at the same time, and further improve the service life and prolong the service time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating protection technology, specifically relating to a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders, and its preparation method. Background Technology

[0002] Carbon steel is a common type of steel, suitable for industrial applications that require bearing significant pressure and weight. However, it is susceptible to moisture, rust, and acid and alkali corrosion.

[0003] Plasma cladding is a surface modification method that uses plasma to heat the surface of a material, melting it and bonding it with the substrate material. Laminating a metallic coating onto carbon steel can significantly improve its corrosion resistance. However, its resistance to chloride ions is insufficient, and its low hardness limits its applications. Medium-entropy / high-entropy alloy coatings can significantly improve corrosion resistance, but they also suffer from low hardness. Currently, the preparation of ultra-hard high-entropy / medium-entropy alloy coatings by plasma cladding mainly involves adding hard phases. However, traditional plasma cladding techniques have some problems in generating reinforcing coatings, such as insufficient bonding between the substrate and hard phases, and microcracks. Furthermore, the decomposition and dilution of medium-entropy / high-entropy alloy powder during plasma cladding can lead to a decrease in the content of medium-entropy / high-entropy phases within the coating, affecting its corrosion resistance. Summary of the Invention

[0004] To address the problems existing in the prior art, the present invention aims to provide a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders, and its preparation method. The present invention can improve the corrosion resistance, hardness and wear resistance of the coating, and obtain a medium-entropy alloy coating with an ultra-hard reinforcing phase.

[0005] The technical solution adopted in this invention is as follows:

[0006] A method for preparing a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders includes the following steps:

[0007] The composite powder was prepared into a cladding layer by plasma cladding, and the cladding layer served as the medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders.

[0008] The composite powder is a mixture of metal powder and ceramic powder;

[0009] When composite powder is prepared into a cladding layer using plasma cladding, a portion of the ceramic powder is completely melted and decomposed, while another portion of the ceramic powder is partially melted and decomposed and / or not melted and decomposed. The melted and decomposed ceramic powder reacts with the metal powder to form a medium-entropy alloy phase.

[0010] The metal powder is a mixture of iron powder, nickel powder and chromium powder.

[0011] Preferably, the metal powder is a mixture of iron powder, nickel powder and chromium powder, wherein the iron powder, nickel powder and chromium powder account for 65% to 69% of the mass of the composite powder, 15% and 10% respectively, and the balance of the composite powder is ceramic powder.

[0012] Preferably, the ceramic powder is one or a mixture of several of zirconium oxide, aluminum oxide, titanium oxide, silicon carbide and chromium carbide.

[0013] Preferably, the particle size of the ceramic powder is 45–120 μm.

[0014] Preferably, the particle size of the metal powder is 30–115 μm.

[0015] Preferably, when preparing the composite powder into a cladding layer using the plasma cladding method, the working current is 90-120A, the scanning speed is 3-5mm / s, the ion gas flow rate is 2.5L / min, and the protective gas flow rate is 15.0L / min.

[0016] Preferably, the preparation method further includes a pretreatment process, which includes drying the composite powder and polishing and cleaning the substrate covered by the cladding layer.

[0017] The present invention also provides a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders. The coating is prepared by the preparation method described above, and the Vickers hardness of the coating is above 400HV0.3.

[0018] Preferably, in the cladding layer, the unmelted and decomposed portion of the ceramic powder is bonded to the entropy-like alloy phase in a metallurgical manner.

[0019] The present invention has the following beneficial effects:

[0020] In the preparation method of this invention, when the composite powder is prepared into a cladding layer using a plasma cladding method, a portion of the ceramic powder completely melts and decomposes, while another portion partially melts and decomposes and / or remains unmelted and undecomposed. The melted and decomposed ceramic powder reacts with the metal powder to form a mid-entropy alloy phase, significantly improving corrosion resistance on the basis of the original metal. The partially melted and / or unmelted particles are distributed in the matrix phase, improving wear resistance. Therefore, the mid-entropy alloy coating prepared by the method of this invention can simultaneously and significantly improve both wear resistance and corrosion resistance, thereby increasing service life and extending service time. Attached Figure Description

[0021] Figure 1 Image showing the wear morphology of a pure stainless steel weld layer;

[0022] Figure 2 This is a wear morphology diagram of the weld layer in Embodiment 1 of the present invention;

[0023] Figure 3 This is a wear morphology diagram of the weld layer in Embodiment 2 of the present invention;

[0024] Figure 4 This is a wear morphology diagram of the weld layer in Embodiment 3 of the present invention. Detailed Implementation

[0025] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0026] This invention discloses a method for preparing a mid-entropy-like alloy coating with an ultra-hard reinforcing phase generated in situ from hard ceramic particles and various metal powders. The method includes the following steps: A composite powder, mechanically mixed with various high-purity metal powders and ceramic powders, is used in a plasma cladding method to generate a mid-entropy-like alloy coating with an ultra-hard reinforcing phase in situ. Specifically, when preparing the cladding layer from the composite powder using plasma cladding, a high-energy ion beam melts and decomposes part of the ceramic powder, which then reacts with metal powders (such as Fe, Cr, and Ni) to generate a mid-entropy-like alloy phase in situ, improving the coating's corrosion resistance. Only the surface-melted and / or unmelted ceramic powder is dispersed as a hard phase in the coating. The bonding between the unmelted hard ceramic particles and the alloy matrix phase is metallurgical. This invention simultaneously introduces unmelted and partially melted ceramic particles into the coating, improving the hardness and wear resistance of the cladding layer, thus obtaining a mid-entropy-like alloy coating with an ultra-hard reinforcing phase.

[0027] The ceramic powder used in the above-mentioned scheme of the present invention comprises one or a mixture of several of zirconium oxide, alumina, titanium oxide, silicon carbide, and chromium carbide. The particle size of the ceramic powder is 45-120 μm, ensuring that small-sized particles melt during cladding, while the surface of large-sized particles melts but the core remains unmelted.

[0028] The metal powder used in the above-mentioned scheme of the present invention comprises a mixture of at least three of iron powder, nickel powder, chromium powder, cobalt powder and aluminum powder, wherein the purity of the metal powder is higher than 99.99% and the particle size of the metal powder is 30-115 μm.

[0029] When preparing the composite powder into a cladding layer using plasma cladding, the working current is 90-120A, the scanning speed is 3-5mm / s, the ion gas flow rate is 2.5L / min, and the protective gas flow rate is 15.0L / min.

[0030] In this invention, ceramic phase particles (i.e., ceramic powder) react with several metal powders to generate a mid-entropy alloy phase and a reinforcing phase. During plasma cladding, plasma parameters are controlled to achieve a melting effect where smaller ceramic particles melt while larger particles partially melt. The ceramic and metal components from the melting and decomposition influence the generation of the mid-entropy alloy phase, significantly improving corrosion resistance on the basis of the original metal. The partially melted particles are distributed in the matrix phase, enhancing wear resistance. Therefore, the mid-entropy alloy coating prepared by this invention can simultaneously and significantly improve both wear resistance and corrosion resistance, thereby increasing service life and extending service time.

[0031] The embodiments of the present invention are carried out using the following raw materials and parameters. It is understood that, inspired by the above principles of the present invention, coatings prepared using other raw materials and parameters are all cases in which the concept of the present invention has been adopted.

[0032] This invention relates to a medium-entropy alloy coating material based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders. The metal powder used in this material is a mixture of iron powder, chromium powder, and nickel powder, and the ceramic powder is ZrO2 powder. By mass percentage, the raw material contains 65%–69% iron, 15% chromium, 10% nickel, and 6%–10% ZrO2 powder. The ZrO2 powder has a particle size of 45–120 μm, and the metal powder has a particle size of 30–115 μm.

[0033] The preparation method of this coating includes the following steps:

[0034] Step 1: Place the metal powder and ZrO2 powder in an oven and dry them at 100°C for 3 hours;

[0035] Step 2: Weigh the metal powder and ZrO2 powder according to the specified ratio and mechanically mix them to form a composite powder.

[0036] Step 3: Prepare the composite powder into a cladding layer using plasma cladding. The parameters for plasma cladding are as follows: working current is 90-120A, scanning speed is 3-5mm / s, ion gas flow rate is 2.5L / min, and protective gas flow rate is 15.0L / min.

[0037] Example 1

[0038] The composite powder in this embodiment comprises: 65% iron, 15% chromium, 10% nickel, and 10% ZrO2 powder. The ZrO2 powder has a particle size of 45–120 μm, and the metal powder has a particle size of 30–115 μm. A cladding layer is prepared on the substrate material using plasma cladding equipment with the following parameters: operating current of 90 A, scanning speed of 3 mm / s, ion gas flow rate of 2.5 L / min, and protective gas flow rate of 15.0 L / min.

[0039] Step 1: Place the different powders into an oven and dry them at 100℃ for 3 hours;

[0040] Step 2: Weigh the powders according to the specified proportions and mix them mechanically;

[0041] Step 3: Select a Q235 substrate, use sandpaper to remove the oxide layer and impurities on the surface of the Q235 board, and use acetone to wipe away oil and water stains on the surface of the Q235.

[0042] Step 4: Place the powder obtained in Step 2 into the powder feeder and feed the powder out with 99.99% Ar;

[0043] Step 5: Prepare a cladding layer on the Q235 surface treated in Step 3 using a plasma cladding method;

[0044] Step 6: The microhardness and wear amount of the stainless steel coating and the weld layer prepared in this embodiment were tested using a hardness tester and a friction and wear testing machine. The hardness test was performed with a load of 300g and a holding time of 10s. A pin-disc type was used for the wear test; the weld layer sample was a cylindrical specimen with a diameter of 4.8mm and a height of 12.7mm. The friction pair was GCr15. The friction and wear test was performed with a load of 50N, a time of 5min, and a rotation speed of 100r / min.

[0045] The coating obtained in this embodiment was tested for hardness and wear resistance. The Vickers hardness was 800 HV 0.3, and the wear amount was 2% of that of the stainless steel coating. The friction and wear morphology of the stainless steel coating is as follows. Figure 1 The friction and wear morphology of the coating in this embodiment is as follows: Figure 2 As shown, under the same wear conditions, the stainless steel coating underwent severe wear, with significant adhesive wear marks on the surface. In this embodiment, the surface of the coating after wear was mainly characterized by a plough-groove morphology, with no adhesive wear marks.

[0046] Example 2

[0047] The composite powder in this embodiment comprises: 67% iron, 15% chromium, 10% nickel, and 8% ZrO2 powder. The ZrO2 powder has a particle size of 45–120 μm, and the metal powder has a particle size of 30–115 μm. A cladding layer is prepared on the substrate material using plasma cladding equipment with the following parameters: operating current of 110 A, scanning speed of 3 mm / s, ion gas flow rate of 2.5 L / min, and protective gas flow rate of 15.0 L / min.

[0048] Step 1: Place the different powders into an oven and dry them at 100℃ for 3 hours;

[0049] Step 2: Weigh the powders according to the specified proportions and mix them mechanically;

[0050] Step 3: Select a Q235 substrate, use sandpaper to remove the oxide layer and impurities on the surface of the Q235 board, and use acetone to wipe away oil and water stains on the surface of the Q235.

[0051] Step 4: Place the powder obtained in Step 2 into the powder feeder and feed the powder out with 99.99% Ar;

[0052] Step 5: Prepare a cladding layer on the Q235 surface treated in Step 3 using a plasma cladding method;

[0053] Step 6: The microhardness and wear amount of the stainless steel coating and the weld layer prepared in this embodiment were tested using a hardness tester and a friction and wear testing machine. The hardness test was performed with a load of 300g and a holding time of 10s. A pin-disc type was used for the wear test; the weld layer sample was a cylindrical specimen with a diameter of 4.8mm and a height of 12.7mm. The friction pair was GCr15. The friction and wear test was performed with a load of 50N, a time of 5min, and a rotation speed of 100r / min.

[0054] The coating obtained in this embodiment was tested for hardness and wear resistance. The Vickers hardness was 500 HV 0.3, and the wear amount was 10% of that of the stainless steel coating. The wear morphology of the coating obtained in this embodiment is as follows. Figure 3 As shown, the coating obtained in this embodiment exhibits a certain number of ploughing grooves and adhesive wear morphology on its surface after wear. However, adhesive wear accounts for a relatively small proportion, with abrasive wear being the dominant type, and the wear is lower than that of the stainless steel coating.

[0055] Example 3

[0056] The composite powder comprises: 69% iron, 15% chromium, 10% nickel, and 6% ZrO2 powder. A cladding layer is prepared on the substrate material using plasma cladding equipment with the following parameters: operating current 120A, scanning speed 5mm / s, ion gas flow rate 2.5L / min, and protective gas flow rate 15.0L / min.

[0057] Step 1: Place the different powders into an oven and dry them at 100℃ for 3 hours;

[0058] Step 2: Weigh the powders according to the specified proportions and mix them mechanically;

[0059] Step 3: Select a Q235 substrate, use sandpaper to remove the oxide layer and impurities on the surface of the Q235 board, and use acetone to wipe away oil and water stains on the surface of the Q235.

[0060] Step 4: Place the powder obtained in Step 2 into the powder feeder and feed the powder out with 99.99% Ar;

[0061] Step 5: Prepare a cladding layer on the Q235 surface treated in Step 3 using a plasma cladding method;

[0062] Step 6: The microhardness and wear amount of the stainless steel coating and the weld layer prepared in this embodiment were tested using a hardness tester and a friction and wear testing machine. The hardness test was performed with a load of 300g and a holding time of 10s. A pin-disc type was used for the wear test; the weld layer sample was a cylindrical specimen with a diameter of 4.8mm and a height of 12.7mm. The friction pair was GCr15. The friction and wear test was performed with a load of 50N, a time of 5min, and a rotation speed of 100r / min.

[0063] The coating obtained in this embodiment was tested for hardness and wear resistance. The Vickers hardness was 400 HV 0.3, and the wear amount was 30% of that of the stainless steel coating. The wear morphology of the coating obtained in this embodiment is as follows. Figure 4 As shown. The wear surface of the coating obtained in this embodiment mainly exhibits ploughing and adhesive wear morphologies. The proportions of the two morphologies are similar, but their wear amount is lower than that of the stainless steel coating.

[0064] As can be seen from the above scheme, this invention has the following characteristics: Based on a mechanically mixed powder of various metals and ceramics, plasma cladding technology can be used to directly prepare a medium-entropy alloy coating with an ultra-hard reinforcing phase on the surface of a carbon steel substrate in an in-situ manner. The added ceramic particles have a wide size range. Small-sized ceramic powders melt and decompose, reacting with the metal to generate a medium-entropy alloy phase in situ; large-sized particles only melt on their surface, acting as a hard phase dispersed in the coating, thus improving the coating's hardness and wear resistance. Compared with metal cladding layers, this patented cladding layer not only improves corrosion resistance but also significantly enhances wear resistance.

[0065] The above embodiments demonstrate that the process of the present invention is simple and feasible, and the superhard medium-entropy alloy cladding layer prepared by the present invention has properties such as high hardness and high wear resistance, which can meet the requirements of extending the service life and long maintenance cycle of wear-resistant parts.

[0066] It should be noted that the above-described embodiments are merely preferred embodiments of the present invention. Besides the above embodiments, the present invention has many other embodiments. All technical solutions formed by equivalent substitutions fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a medium-entropy alloy coating based on the in-situ formation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders, characterized in that, The process includes the following: A cladding layer is prepared from composite powder using a plasma cladding method. The cladding layer serves as a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders. In the cladding layer, the unmelted and decomposed portion of the ceramic powder is bonded to the medium-entropy alloy-like phase in a metallurgical manner. The composite powder is a mixture of metal powder and ceramic powder; the metal powder is a mixture of iron powder, nickel powder and chromium powder; the iron powder, nickel powder and chromium powder account for 65%~69%, 10% and 15% of the mass of the composite powder, respectively, and the balance of the composite powder is ceramic powder; the ceramic powder is zirconium oxide. When preparing a cladding layer from composite powder using plasma cladding, the working current is 90~120A and the scanning speed is 3~5mm / s; a portion of the ceramic powder is completely melted and decomposed, while another portion of the ceramic powder is partially melted and decomposed and / or not melted and decomposed. The melted and decomposed ceramic powder and metal powder form a medium-entropy alloy phase. The particle size of the ceramic powder is 45~120μm; The particle size of the metal powder is 30~115μm.

2. The method for preparing a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders according to claim 1, characterized in that, When the composite powder is prepared into a cladding layer using the plasma cladding method, the ion gas flow rate is 2.5 L / min and the protective gas flow rate is 15.0 L / min.

3. The method for preparing a medium-entropy alloy coating based on the in-situ generation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders according to claim 1, characterized in that, It also includes a pretreatment process, which includes drying the composite powder and polishing and cleaning the substrate covered by the cladding layer.

4. A medium-entropy alloy coating based on the in-situ formation of an ultra-hard reinforcing phase from hard ceramic particles and various metal powders, characterized in that, The coating is prepared by the preparation method described in any one of claims 1-3, and the Vickers hardness of the coating is 400HV0.3 or higher; in the cladding layer, the unmelted and decomposed part of the ceramic powder is bonded to the medium-entropy alloy phase in a metallurgical manner.