Conductive paste, conductive trace, and solar cell
By combining four types of spherical metal powders with different particle sizes, the problems of high aspect ratio and flowability in the conductive silver paste printing process were solved, and conductive traces with high plasticity and low resistance were prepared, thereby improving the photoelectric conversion efficiency of solar cells.
Patent Information
- Application Number
- CN202311846559.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing conductive silver paste printing processes are difficult to improve the aspect ratio, resulting in a large shading area, which affects the photoelectric conversion efficiency of heterojunction solar cells. Furthermore, the high fluidity of conductive pastes on the market leads to poor line shapes after printing.
Conductive pastes with high plasticity are prepared by using four types of spherical metal powders with different particle sizes, including nano-sized, submicron-sized, and micron-sized powders, and by adjusting the powder ratio and components such as organic carriers and curing agents. This paste is suitable for fine-line printing.
Conductive traces with an aspect ratio greater than or equal to 0.5 and a volume resistivity less than or equal to 6×10⁻⁶ were achieved, improving the photoelectric conversion efficiency of solar cells.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of materials technology, specifically to conductive pastes, conductive traces, and solar cells. Background Technology
[0002] Currently, the most commonly used grid electrodes are made of screen-printed conductive silver paste. However, the printing process struggles to further improve their aspect ratio, resulting in a large light-blocking area. When applied to heterojunction solar cells, this affects the cell's light absorption, thus impacting photoelectric conversion efficiency. Furthermore, the high fluidity of commercially available global powder-based conductive pastes leads to poor line shaping capabilities after printing, causing the lines to collapse on the cell and become wide and low.
[0003] In recent years, in order to improve the aspect ratio of printing pastes, the industry has also taken some measures, such as compounding epoxy resin, polyurethane and aliphatic epoxy resin, adjusting the viscosity of organic carrier, and effectively improving the plasticity of paste, but there are printability problems; another example is to use composite electrodes, with silver-coated copper paste as the base film layer and pure silver paste as the cover layer, but there are problems such as complex preparation process. Summary of the Invention
[0004] This invention aims to at least partially solve one of the technical problems in the related art. To this end, one object of this invention is to provide a conductive paste that can be printed to produce conductive traces with a large aspect ratio.
[0005] In one aspect of the present invention, a conductive paste is provided. According to an embodiment of the present invention, the conductive paste comprises: 92-94 parts by weight of spherical metal powder; 2-5 parts by weight of an organic carrier; 1.5-3 parts by weight of a solvent; 0.1-1 parts by weight of a curing agent; and 0.1-1 parts by weight of an additive, wherein the metal powder comprises a first metal powder, a second metal powder, a third metal powder, and a fourth metal powder, wherein the average particle size D50 of the first metal powder is 100-200 nm, the average particle size D50 of the second metal powder is 0.3-0.5 μm, the average particle size D50 of the third metal powder is 0.5-0.8 μm, and the average particle size D50 of the fourth metal powder is 2-4 μm. Therefore, the metal powder includes four types of spherical metal powders with different particle sizes: a first metal powder of nanoparticle size, a second and third metal powder of submicron size, and a fourth metal powder of micron size. The combination of these four types of spherical metal powders with different particle sizes enables the global powder system (i.e., all four metal powders are spherical powders) conductive paste of the present invention to achieve dense stacking, resulting in strong plasticity of the conductive paste. This helps to maintain the plasticity of the conductive lines prepared from the conductive paste, thereby facilitating the preparation of conductive lines with higher aspect ratios and / or lower volume resistivity, which in turn helps to improve the photoelectric conversion efficiency of solar cells using the conductive lines. Moreover, the above-mentioned conductive paste can also be used for fine line printing with openings of 18 μm and below.
[0006] According to an embodiment of the present invention, the first metal powder also satisfies at least one of the following conditions: the tap density of the first metal powder is less than or equal to 1.5 g / cc; the first metal powder is silver powder and is in a dry and fluffy state.
[0007] According to an embodiment of the present invention, the second metal powder further satisfies at least one of the following conditions: the D10 particle size of the second metal powder is 0.1~0.5μm; the D90 particle size of the second metal powder is 0.6~1.0μm; the tap density of the second metal powder is less than or equal to 6g / cc; and the second metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder.
[0008] According to an embodiment of the present invention, the third metal powder further satisfies at least one of the following conditions: the D10 particle size of the third metal powder is 0.2~0.6μm; the D90 particle size of the third metal powder is 0.6~1.0μm; the tap density of the third metal powder is less than or equal to 6g / cc; and the third metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder.
[0009] According to an embodiment of the present invention, the fourth metal powder further satisfies at least one of the following conditions: the D10 particle size of the fourth metal powder is 1~3μm; the D90 particle size of the fourth metal powder is 4~7μm; the D90 / D50 ratio is 1.0~4.0; the tap density of the fourth metal powder is less than or equal to 5g / cc; the fourth metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder, optionally, the fourth metal powder is silver-coated copper powder, and the silver coating content is 20~40%.
[0010] According to an embodiment of the present invention, based on the total mass of the spherical metal powder, the mass ratio of the first metal powder, the second metal powder, the third metal powder and the fourth metal powder is 1~10:10~20:10~30:60~80, preferably 1~4:10~15:15~25:60~70.
[0011] According to an embodiment of the present invention, the conductive paste further satisfies at least one of the following conditions: the organic carrier comprises a bisphenol-type epoxy resin and an epoxy diluent, wherein the bisphenol-type epoxy resin comprises at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, hydrogenated bisphenol A type epoxy resin, and hydrogenated bisphenol F type epoxy resin, and the mass fraction of the epoxy diluent is 25%~35% based on the total mass of the organic carrier; the curing agent comprises imidazole, 2-methylimidazolium, 2-ethyl-4-methylimidazolium, 2-undecylimidazolium, 2- The additives include at least one of the following: heptadecanidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-aminoethyl-2-methylimidazole, 1-methylimidazole, 2-ethylimidazole, etc.; boron trifluoride ethyl ether; boron trifluoride phenol; boron trifluoride piperidine; boron trifluoride acetate; boron trifluoride monomethylamine; boron trifluoride monoethylamine; boron trifluoride triethanolamine; and boron trifluoride monoethanolamine; the additives include at least one of the following: stabilizers, silane coupling agents, dispersants, leveling agents, antioxidants, defoamers, and viscosity modifiers.
[0012] According to an embodiment of the present invention, under the conditions of 25°C and 10 r / min, the viscosity of the conductive paste is 50~600 Pa·s, preferably 200~350 Pa·s.
[0013] In another aspect, the present invention provides a conductive trace. According to an embodiment of the present invention, the conductive trace is prepared from the conductive paste described above, and the conductive trace satisfies at least one of the following conditions: the aspect ratio of the conductive trace is greater than or equal to 0.5; the volume resistivity of the conductive trace is less than or equal to 6 × 10⁻⁶. -6Therefore, this conductive trace has a full linearity, a relatively high aspect ratio, and a low volume resistivity. Applying it to solar cells can help improve the photoelectric conversion efficiency of solar cells.
[0014] In another aspect, the present invention provides a solar cell, according to an embodiment of the invention, comprising grid lines, said grid lines being the conductive traces described above. Therefore, the solar cell exhibits high photoelectric conversion efficiency. Those skilled in the art will understand that this solar cell possesses all the features and advantages of the conductive traces and conductive paste described above, and will not be elaborated further here. Detailed Implementation
[0015] The present invention will be explained below with reference to embodiments. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0016] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.
[0017] In one aspect of the invention, a conductive paste is provided. According to an embodiment of the invention, the conductive paste comprises: 92-94 parts by weight of spherical metal powder; 2-5 parts by weight of an organic carrier; 1.5-3 parts by weight of a solvent; 0.1-1 parts by weight of a curing agent; and 0.1-1 parts by weight of an additive, wherein the metal powder comprises a first metal powder, a second metal powder, a third metal powder, and a fourth metal powder, and the average particle size D50 of the first metal powder is 100-200 nm (e.g., 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm). The average particle size D50 of the second metal powder is 0.3~0.5μm (e.g., 0.3μm, 0.32μm, 0.34μm, 0.35μm, 0.36μm, 0.38μm, 0.4μm, 0.42μm, 0.44μm, 0.46μm, 0.48μm, 0.5μm, etc.), and the average particle size D50 of the third metal powder is 0.5~0.8μm (e.g., 0.5μm, 0.52μm, etc.). The average particle size D50 of the fourth metal powder is 2~4μm (e.g., 2μm, 2.2μm, 2.5μm, 2.8μm, 3.0μm, 3.2μm, 3.5μm, 3.7μm, 4.0μm, etc.). Therefore, the metal powder comprises four types of spherical metal powders with different particle sizes: a first metal powder of nanoparticle size, a second and third metal powder of submicron size, and a fourth metal powder of micron size. The combination of these four types of spherical metal powders with different particle sizes enables the global powder system (i.e., all four metal powders are spherical powders) conductive paste of the present invention to achieve dense packing (small-diameter metal powders can fill the gaps between large-diameter metal powders), resulting in strong plasticity of the conductive paste. This helps to maintain the plasticity of the conductive lines prepared from the conductive paste, thereby facilitating the preparation of conductive lines with higher aspect ratios and / or lower volume resistivity, which in turn helps to improve the photoelectric conversion efficiency of solar cells using the conductive lines. Moreover, the above-mentioned conductive paste can also be used for fine line printing with apertures of 18 μm and below.
[0018] The amount of curing agent used is 0.1-1 parts by mass, which is beneficial for the effective film formation of the conductive paste after printing, resulting in better adhesion of the printed conductive lines. If the amount of curing agent is less than 0.1 parts by mass, the coupling agent in the additives may not fully open its ring, failing to react with the organic carrier. This may lead to insufficient adhesion of the cured material (electrodes or wiring, etc.) after printing. In addition, the number of strongly coordinating atoms in the cured material (electrodes, wiring, etc.) may be small, failing to achieve the goal of reducing contact resistance. On the other hand, if the amount of curing agent exceeds 1 part by mass, the viscosity of the conductive paste may be too high, posing a risk of printing defects. Furthermore, the amount of solvent used can give the conductive paste suitable viscosity and fluidity. If the amount of solvent is too large, the viscosity of the conductive paste will be relatively high, resulting in relatively poor forming ability. If the amount of solvent is too small, the viscosity of the paste will be relatively high, easily causing the conductive paste to lose the shear fluidity required for the printing process, making it difficult to print.
[0019] According to some embodiments of the present invention, the tap density of the first metal powder is less than or equal to 1.5 g / cc, which is beneficial for the dense stacking of the metal powder, improves the plasticity of the conductive paste, and helps maintain the plasticity of the conductive traces prepared from the conductive paste, thereby facilitating the preparation of conductive traces with higher aspect ratios and / or lower volume resistivity. According to some embodiments of the present invention, the first metal powder is silver powder. Furthermore, the first metal powder is in a dry and fluffy state, possessing high activity and low-temperature sintering characteristics.
[0020] According to some embodiments of the present invention, the D10 particle size of the second metal powder is 0.1~0.5μm, such as 0.1μm, 0.15μm, 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.45μm, 0.5μm, etc. According to some embodiments of the present invention, the D90 particle size of the second metal powder is 0.6~1.0μm, such as 0.6μm, 0.65μm, 0.7μm, 0.75μm, 0.8μm, 0.85μm, 0.9μm, 0.95μm, 1.0μm, etc. The second metal powder with the above-mentioned particle size can be fully mixed with the first metal powder and is not prone to agglomeration. According to some embodiments of the present invention, the tap density of the second metal powder is less than or equal to 6 g / cc, which is beneficial for the dense stacking of the metal powder, improves the plasticity of the conductive paste, and helps maintain the plasticity of the conductive traces prepared from the conductive paste, thereby facilitating the preparation of conductive traces with higher aspect ratios and / or lower volume resistivity. According to some embodiments of the present invention, the second metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder. The above materials have better conductivity.
[0021] According to some embodiments of the present invention, the D10 particle size of the third metal powder is 0.2~0.6 μm, such as 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, etc. The D90 particle size of the third metal powder is 0.6~1.0 μm, such as 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1.0 μm, etc. The third metal powder with the above-mentioned particle size can be fully mixed and tightly packed with the first metal powder, the second metal powder, etc., and is not prone to agglomeration. The tap density of the third metal powder is less than or equal to 6 g / cc. The third metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder.
[0022] According to some embodiments of the present invention, the D10 particle size of the fourth metal powder is 1~3μm, such as 1μm, 1.2μm, 1.5μm, 1.8μm, 2.0μm, 2.2μm, 2.5μm, 2.7μm, 3.0μm, etc. The D90 particle size of the fourth metal powder is 4~7μm, such as 4μm, 4.5μm, 5μm, 5.5μm, 6.0μm, 6.5μm, 7μm, etc. The D90 / D50 ratio is 1.0 to 4.0, for example, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, or 4.0; the tap density of the fourth metal powder is less than or equal to 5 g / cc; the fourth metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, or silver-coated aluminum powder, and further, the fourth metal powder is silver-coated copper powder with a silver coating of 20 to 40%.
[0023] According to an embodiment of the present invention, based on the total mass of the spherical metal powder, the mass ratio of the first metal powder, the second metal powder, the third metal powder, and the fourth metal powder is 1~10:10~20:10~30:60~80. The metal powder in the above ratio can make the conductive paste have a suitable viscosity, which is convenient for printing conductive lines and can obtain conductive lines with suitable resistance. It is also beneficial for small-diameter metal powder to fully fill the pores generated between large-diameter metal powder.
[0024] In some specific embodiments, the mass ratio of the first metal powder, the second metal powder, the third metal powder, and the fourth metal powder is 1~4:10~15:15~25:60~70. Within this range, a conductive paste with better performance can be obtained. If the amount of the first metal powder is greater than 4 parts by mass, the viscosity of the conductive paste will increase relatively, resulting in poor screen printing properties of the cured product (i.e., conductive traces, such as electrodes, wiring, etc.). On the other hand, if the amount of the first metal powder is less than 1 part by mass, the contact resistance of the cured product will be relatively high. For submicron-sized second and third metal powders, the mass ratio is 10-15:15-25. If the amount of second metal powder is less than 10 parts by mass, the proportion of large-sized third metal powder will be too high, resulting in insufficient filling of the gaps between the large-sized third and fourth metal powders, leading to a high volume resistivity of the printed cured material. On the other hand, if the amount of third metal powder is less than 15 parts by mass, the proportion of small-sized second metal powder will be too high, potentially causing excessively high paste viscosity and poor printability, thus failing to meet the requirements for ultra-fine line printing. If the amount of fourth metal powder is greater than 70 parts by mass, it can easily lead to poor filling of the conductive paste with the substrate during printing and is not suitable for small textured heterojunction solar cells, resulting in a sharp increase in contact resistance. On the other hand, if the amount of fourth metal powder is less than 60 parts by mass, the amount of silver powder required to prepare the same mass of paste is too high, i.e., the cost is higher, failing to meet the cost reduction requirements.
[0025] According to some embodiments of the present invention, the organic carrier can be a thermosetting organic carrier, comprising a bisphenol-type epoxy resin and an epoxy diluent. The bisphenol-type epoxy resin includes at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, hydrogenated bisphenol A type epoxy resin, and hydrogenated bisphenol F type epoxy resin. Based on the total mass of the organic carrier, the mass fraction of the epoxy diluent is 25% to 35%, such as 25%, 28%, 30%, 32%, 35%, etc. This proportion of organic carrier is beneficial for the printing of conductive paste and the formation of conductive lines. If too much epoxy diluent is added, the printed conductive lines will collapse; if too little epoxy diluent is added, or even none is added, the conductive paste will have excessive stringing, failing to meet printing requirements.
[0026] According to some embodiments of the present invention, the curing agent can be a cationic curing agent containing nitrogen or fluorine atoms, including at least one of imidazoles, 2-methylimidazolium, 2-ethyl-4-methylimidazolium, 2-undecylimidazolium, 2-heptadecylimidazolium, 1-benzyl-2-methylimidazolium, 2-phenyl-4-methylimidazolium, 1-cyanoethyl-2-methylimidazolium, 1-aminoethyl-2-methylimidazolium, 1-methylimidazolium, 2-ethylimidazolium, etc., boron trifluoride ethyl ether, boron trifluoride phenol, boron trifluoride piperidine, boron trifluoride acetate, boron trifluoride monomethylamine, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride monoethanolamine. The selection of the above-mentioned curing agent is beneficial to the printing and molding of the conductive paste, resulting in conductive traces with better adhesion.
[0027] According to some embodiments of the present invention, the additives include at least one of stabilizers, silane coupling agents, dispersants, leveling agents, antioxidants, defoamers, and viscosity modifiers. This can further improve the performance of the conductive paste.
[0028] According to some embodiments of the present invention, the solvent may be selected from saturated hydrocarbon solvents such as hexane, aromatic hydrocarbon solvents such as toluene, glycol ether (solvent) solvents such as ethyl cellosolve, butyl cellosolve, and butyl cellosolve acetate, glycol ether solvents such as diethylene glycol diethyl ether and butyl carbitol (diethylene glycol monobutyl ether), acetate solvents such as diethylene glycol butyl ether acetate and carbitol butyl ether acetate, alcohol solvents such as diacetone alcohol, terpineol, and benzyl alcohol, ketone solvents such as cyclohexanone and methyl ethyl ketone, and ester solvents such as DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyl ester, and 2,2,4-trimethyl-1,3-pentanediol diisobutyl ester.
[0029] According to embodiments of the present invention, under conditions of 25°C and 10 r / min, the viscosity of the conductive paste is 50~600 Pa·s, for example, 50 Pa·s, 100 Pa·s, 150 Pa·s, 200 Pa·s, 250 Pa·s, 300 Pa·s, 350 Pa·s, 400 Pa·s, 450 Pa·s, 500 Pa·s, 550 Pa·s, 600 Pa·s, etc. Conductive pastes with the above viscosities facilitate the printing process. In some specific embodiments, the viscosity of the conductive paste is 200~350 Pa·s.
[0030] In another aspect, the present invention provides a conductive trace. According to an embodiment of the present invention, the conductive trace is prepared from the conductive paste described above, and the conductive trace satisfies at least one of the following conditions: the aspect ratio of the conductive trace is greater than or equal to 0.5; the volume resistivity of the conductive trace is less than or equal to 6 × 10⁻⁶. -6Therefore, this conductive trace has a relatively high aspect ratio and low volume resistivity, which helps to improve the photoelectric conversion efficiency of solar cells when applied to them.
[0031] According to an embodiment of the present invention, when mixing the various components in the conductive paste, a planetary mixer, a three-roll mill, or other mixing equipment is used.
[0032] According to embodiments of the present invention, when preparing conductive traces using conductive paste, printing methods such as screen printing, gravure printing, offset printing, inkjet printing, distributor printing, and immersion printing can be used.
[0033] According to an embodiment of the present invention, the wire routing can be a collector (such as a grid line) in a solar cell, an internal or external electrode of a chip-type electronic component, or an electrode, wiring, or bonding of a component used in electromagnetic wave shielding, vibrator bonding, membrane switches, touch panels, etc.
[0034] In another aspect, the present invention provides a solar cell, according to an embodiment of the invention, comprising grid lines, said grid lines being the conductive traces described above. Thus, the grid lines have a high aspect ratio, which is beneficial for improving the photoelectric conversion efficiency of the solar cell. Those skilled in the art will understand that this solar cell possesses all the features and advantages of the conductive traces and conductive paste described above, and will not be elaborated further.
[0035] According to embodiments of the present invention, there are no special requirements for the specific type of solar cell, and those skilled in the art can flexibly select it according to actual needs. In some embodiments, the solar cell can be a heterojunction solar cell, a PERC solar cell, or an IBC solar cell.
[0036] Example Example 1 (1) The conductive paste comprises 1.6 parts by weight of a first metal powder, 5 parts by weight of a second metal powder, 24 parts by weight of a third metal powder, 62 parts by weight of a fourth metal powder, 1.4 parts by weight of bisphenol F epoxy resin, 0.8 parts by weight of epoxy diluent, 0.2 parts by weight of cationic curing agent, 0.4 parts by weight of end-capped isocyanate curing agent, 2.5 parts by weight of diethylene glycol butyl ether acetate, 0.08 parts by weight of dispersant, and 0.02 parts by weight of stabilizer. After premixing the above raw materials using a planetary agitator degasser, the paste is rolled into a low-temperature conductive paste with a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s using a three-roll mill. The first metal powder is nano-silver powder with an average particle size D50 of 100 nm; the second metal powder is silver powder with an average particle size D50 of 0.4 μm; the third metal powder is silver powder with an average particle size D50 of 0.5 μm; and the fourth metal powder is silver-coated copper powder with an average particle size D50 of 4 μm.
[0037] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0038] Example 2 (1) The conductive paste comprises 1.6 parts by weight of a first metal powder, 13 parts by weight of a second metal powder, 16 parts by weight of a third metal powder, 62 parts by weight of a fourth metal powder, 1.4 parts by weight of bisphenol F epoxy resin, 0.8 parts by weight of epoxy diluent, 0.2 parts by weight of cationic curing agent, 0.4 parts by weight of end-capped isocyanate curing agent, 2.5 parts by weight of diethylene glycol butyl ether acetate, 0.08 parts by weight of dispersant, and 0.02 parts by weight of stabilizer. After premixing the above raw materials using a planetary agitator degasser, the paste is rolled into a low-temperature conductive paste with a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s using a three-roll mill. The first metal powder is nano-silver powder with an average particle size D50 of 100 nm; the second metal powder is silver powder with an average particle size D50 of 0.2 μm; the third metal powder is silver powder with an average particle size D50 of 0.8 μm; and the fourth metal powder is silver-coated copper powder with an average particle size D50 of 3.5 μm.
[0039] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0040] Example 3 (1) The conductive paste comprises 1.6 parts by weight of a first metal powder, 15 parts by weight of a second metal powder, 25 parts by weight of a third metal powder, 52 parts by weight of a fourth metal powder, 1.4 parts by weight of bisphenol F epoxy resin, 0.8 parts by weight of epoxy diluent, 0.2 parts by weight of cationic curing agent, 0.4 parts by weight of end-capped isocyanate curing agent, 2.5 parts by weight of diethylene glycol butyl ether acetate, 0.08 parts by weight of dispersant, and 0.02 parts by weight of stabilizer. After premixing the above raw materials using a planetary agitator degasser, the paste is rolled into a low-temperature conductive paste with a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s using a three-roll mill. The first metal powder is nano-silver powder with an average particle size D50 of 200 nm; the second metal powder is silver powder with an average particle size D50 of 0.3 μm; the third metal powder is silver powder with an average particle size D50 of 0.6 μm; and the fourth metal powder is silver-coated copper powder with an average particle size D50 of 3.5 μm.
[0041] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0042] Example 4 (1) The conductive paste comprises 1.6 parts by weight of a first metal powder, 13 parts by weight of a second metal powder, 16 parts by weight of a third metal powder, 62 parts by weight of a fourth metal powder, 1.4 parts by weight of bisphenol F epoxy resin, 0.8 parts by weight of epoxy diluent, 0.2 parts by weight of cationic curing agent, 0.4 parts by weight of end-capped isocyanate curing agent, 2.5 parts by weight of diethylene glycol butyl ether acetate, 0.08 parts by weight of dispersant, and 0.02 parts by weight of stabilizer. After premixing the above raw materials using a planetary agitator degasser, the paste is rolled into a low-temperature conductive paste with a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s using a three-roll mill. The first metal powder is nano-silver powder with an average particle size D50 of 150 nm; the second metal powder is silver powder with an average particle size D50 of 0.3 μm; the third metal powder is silver powder with an average particle size D50 of 0.6 μm; and the fourth metal powder is silver-coated copper powder with an average particle size D50 of 2.0 μm.
[0043] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0044] Comparative Example 1 (1) The conductive paste comprises 2 parts by mass of a first metal powder, 29 parts by mass of a second metal powder, 62 parts by mass of a fourth metal powder, 1.4 parts by mass of bisphenol F epoxy resin, 0.8 parts by mass of epoxy diluent, 0.2 parts by mass of cationic curing agent, 0.4 parts by mass of end-capped isocyanate curing agent, 2.5 parts by mass of diethylene glycol butyl ether acetate, 0.08 parts by mass of dispersant, and 0.02 parts by mass of stabilizer. The above raw materials are premixed using a planetary agitator degassing machine and then rolled into a low-temperature conductive paste with a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s using a three-roll mill. The first metal powder is nano silver powder with an average particle size D50 of 100 nm; the second metal powder is silver powder with an average particle size D50 of 0.5 μm; and the fourth metal powder is silver-coated copper powder with an average particle size D50 of 4.0 μm.
[0045] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0046] Comparative Example 2 (1) The conductive paste comprises 31 parts by weight of a third metal powder, 62 parts by weight of a fourth metal powder, 1.4 parts by weight of bisphenol F epoxy resin, 0.8 parts by weight of epoxy diluent, 0.2 parts by weight of cationic curing agent, 0.4 parts by weight of end-capped isocyanate curing agent, 2.5 parts by weight of diethylene glycol butyl ether acetate, 0.08 parts by weight of dispersant, and 0.02 parts by weight of stabilizer. The above raw materials are premixed using a planetary agitator degasser and then rolled using a three-roll mill to a fineness of less than 5 μm and a viscosity in the range of 200-350 Pa·s to form a low-temperature conductive paste. The third metal powder is silver powder with an average particle size D50 of 0.6 μm; the fourth metal powder is silver-coated copper powder with an average particle size D50 of 4.0 μm.
[0047] (2) Using a screen printing machine, the conductive paste was printed on the TCO / Si substrate according to the design pattern of the heterojunction solar cell unit at a squeegee pressure of 0.18MPa and a printing speed of 300mm / s. The paste was dried at 170℃ and cured at 200℃ to form the grid lines of the heterojunction solar cell unit. A total of 200 pieces were produced.
[0048] The viscosity of the conductive paste and the volume resistivity (average value) of the printed grid lines in Examples 1-4 and Comparative Examples 1-2 were tested. The test results are shown in Table 1. The test method is as follows: 1. Viscosity test method: Using conductive slurry as sample, viscosity test is performed using a rotational viscometer at 25℃ with a 14S rotor. When the rotation speed is 10 r / min, the reading time is 4 min to obtain the viscosity of the conductive slurry.
[0049] 2. Volume Resistivity Test: A four-probe ohmmeter was used to test the resistance at both ends of the grid lines. The grid lines are heterojunction solar cells formed on a TCO substrate printed with conductive paste. The specific measurement process is as follows: the resistance between two points is measured using a resistance meter, and then the width, height, and cross-sectional area of the grid lines are measured using a 3D microscope. The volume resistivity result is calculated according to the following formula: Volume resistivity = Resistance / Grid line length × Grid line cross-sectional area / 100 = Line resistance × Grid line cross-sectional area / 100.
[0050] Table 1
[0051] As shown in Table 1, the aspect ratios of the grid lines printed using the conductive pastes of the four particle size combinations are all higher than those obtained using the pastes of two and three particle size combinations. Test data from Examples 2-4 show that the average particle sizes of the submicron-sized second and third metal powders are optimal in the ranges of 0.2-0.3 μm and 0.5-0.6 μm, respectively; increasing the aspect ratio leads to a decrease in volume resistivity.
[0052] Compared with Example 1 and Example 2, after the proportion of the second metal powder is reduced, the proportion of the relatively large-sized third metal powder is increased, the volume resistivity of the gate line prepared by the conductive paste becomes larger, and the minimum matching opening is 20μm.
[0053] Compared to Comparative Example 2, Comparative Example 1, which added nano-silver powder, showed little difference in aspect ratio after printing with low-temperature conductive paste, but the volume resistivity of the grid lines prepared with the low-temperature paste was reduced. This shows that the addition of nano-sized first metal powder helps to reduce the volume resistivity of the grid lines.
[0054] The terms "first" and "second" used in this document are for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature marked "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0055] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0056] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A conductive paste, characterized in that, include: 92-94 parts by weight of spherical metal powder; 2-5 parts by weight of organic carrier; 1.5-3 parts by weight of solvent; 0.1-1 parts by weight of curing agent; 0.1-1 parts by weight of additive, The metal powder includes a first metal powder, a second metal powder, a third metal powder, and a fourth metal powder. The average particle size D50 of the first metal powder is 100~200 nm, the average particle size D50 of the second metal powder is 0.3~0.5 μm, the average particle size D50 of the third metal powder is greater than 0.5 μm and less than or equal to 0.8 μm, and the average particle size D50 of the fourth metal powder is 2~4 μm. The fourth metal powder is silver-coated copper powder; Based on the total mass of the spherical metal powder, the mass ratio of the first metal powder, the second metal powder, the third metal powder, and the fourth metal powder is 1~4:10~15:15~25:60~70.
2. The conductive paste according to claim 1, characterized in that, The first metal powder also satisfies at least one of the following conditions: The tap density of the first metal powder is less than or equal to 1.5 g / cc; The first metal powder is nano silver powder; The first metal powder is in a dry and fluffy state.
3. The conductive paste according to claim 1, characterized in that, The second metal powder also satisfies at least one of the following conditions: The D10 particle size of the second metal powder is 0.1~0.5μm; The D90 particle size of the second metal powder is 0.6~1.0μm; The tap density of the second metal powder is less than or equal to 6 g / cc; The second metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder.
4. The conductive paste according to claim 1, characterized in that, The third metal powder also satisfies at least one of the following conditions: The D10 particle size of the third metal powder is 0.2~0.6μm; The D90 particle size of the third metal powder is 0.6~1.0μm; The tap density of the third metal powder is less than or equal to 6 g / cc; The third metal powder is at least one of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, and silver-coated aluminum powder.
5. The conductive paste according to claim 1, characterized in that, The fourth metal powder also satisfies at least one of the following conditions: The D10 particle size of the fourth metal powder is 1~3μm; The D90 particle size of the fourth metal powder is 4~7μm; The D90 / D50 ratio is 1.0~4.0; The tap density of the fourth metal powder is less than or equal to 5 g / cc; The fourth metal powder has a silver coating content of 20-40%.
6. The conductive paste according to claim 1, characterized in that, It also meets at least one of the following conditions: The organic carrier comprises a bisphenol-type epoxy resin and an epoxy diluent, wherein the bisphenol-type epoxy resin comprises at least one of bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, hydrogenated bisphenol A type epoxy resin, and hydrogenated bisphenol F type epoxy resin, and the epoxy diluent has a mass fraction of 25% to 35% based on the total mass of the organic carrier; The curing agent comprises at least one of imidazole, 2-methylimidazolium, 2-ethyl-4-methylimidazolium, 2-undecylimidazolium, 2-heptadecanylimidazolium, 1-benzyl-2-methylimidazolium, 2-phenyl-4-methylimidazolium, 1-cyanoethyl-2-methylimidazolium, 1-aminoethyl-2-methylimidazolium, 1-methylimidazolium, 2-ethylimidazolium, boron trifluoride ethyl ether, boron trifluoride phenol, boron trifluoride piperidine, boron trifluoride acetate, boron trifluoride monomethylamine, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride monoethanolamine. The additives include at least one of stabilizers, silane coupling agents, dispersants, leveling agents, antioxidants, defoamers, and viscosity modifiers.
7. The conductive paste according to any one of claims 1 to 6, characterized in that, At 25℃ and 10r / min, the viscosity of the conductive paste is 50~600Pa·s.
8. The conductive paste according to claim 7, characterized in that, At 25℃ and 10r / min, the viscosity of the conductive paste is 200~350Pa·s.
9. A conductive trace, characterized in that, The conductive trace is prepared from the conductive paste according to any one of claims 1 to 8, and the conductive trace satisfies at least one of the following conditions: The aspect ratio of the conductive trace is greater than or equal to 0.5; The volume resistivity of the conductive trace is less than or equal to 6 × 10⁻⁶. -6 .
10. A solar cell, characterized in that, Includes a gate line, wherein the gate line is the conductive trace as described in claim 9.
Citation Information
Patent Citations
Low-temperature curing conductive silver paste for laser transfer printing and preparation method thereof
CN115831440A
Low-temperature slurry and heterojunction battery
CN116052923A