Alloy wire and method of making same
By combining nitrogen, phosphorus, and silicon-containing flame retardants with aluminum alloy wire cores, the problems of poor flame retardancy and the influence of hydrogen impurities during the production process were solved. This resulted in highly efficient flame retardancy, stability, and excellent mechanical properties of the alloy wires, reduced burn-off value, and improved conductivity.
Patent Information
- Application Number
- CN202311792272.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-25
AI Technical Summary
Existing alloy wires have poor and unstable flame retardant effects. Hydrogen and harmful impurities during the production process affect product quality. The mechanical and electrical properties of alloy wires are not high, and the burn-off value is high during the aluminum alloy smelting process.
Flame retardants containing nitrogen, phosphorus, and silicon are combined with aluminum alloy wire cores. The flame retardants are prepared through a specific chemical reaction. Combined with rotary blowing degassing and refining agent refining of aluminum liquid, multi-strand aluminum alloy wire cores are prepared. The cores are then wrapped with a polyethylene resin insulation layer and alloy wires are produced using an extrusion process.
This improved the flame retardant properties and stability of the alloy wires, reduced the burn loss value, enhanced mechanical and electrical properties, and ensured product quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of alloy materials technology, specifically relating to an alloy wire and its preparation method. Background Technology
[0002] Alloy wires are mainly used in the field of wires and cables. Wires and cables are widely used and play a vital role in various industrial and mining enterprises, transportation, and other locations. Flame-retardant cables have become the primary choice for cables used in these locations because, in the event of a fire, the dense population and complex building structures make evacuation and rescue operations extremely difficult. Although existing technologies have begun to use halogen-free flame-retardant cable materials, the flame retardants used are usually physically mixed into the matrix, and therefore gradually lose their effectiveness due to external environmental influences. The flame-retardant performance still needs further improvement.
[0003] Currently, copper resources are scarce, and copper mine production capacity is severely insufficient, only able to meet about 30% of market demand. This is extremely detrimental to the development of the wire and cable industry. Aluminum is the most abundant material in the Earth's crust. It has high electrical and thermal conductivity, good corrosion resistance, and good processability. Its density is only about one-third that of copper. Therefore, cables made using aluminum and its alloys weigh half as much as copper cables of the same current carrying capacity. Replacing copper cables with aluminum alloy cables can greatly reduce cable weight, simplify installation, reduce wear, and significantly lower costs. However, the conductivity of aluminum and aluminum alloys is only 61% that of copper.
[0004] Furthermore, due to the simple atomic structure and small atomic radius of hydrogen, it dissolves readily in molten aluminum alloys under normal smelting conditions. However, as the molten aluminum alloy begins to solidify, the solubility of hydrogen decreases sharply, forcing it to precipitate as a gas. After solidification, the gas that fails to leave the molten aluminum alloy remains in the casting, forming defects such as porosity or shrinkage. These defects severely weaken the casting's strength, corrosion resistance, and conductivity, affecting surface quality and increasing the scrap rate. In addition, other factors during production also affect burn-off. Higher slag content results in a higher burn-off value and higher costs. Industrially, it's impractical to avoid or minimize slag removal to reduce burn-off, as this would severely impact the quality of the molten aluminum and significantly harm product quality. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an alloy wire and its preparation method. It solves the problems of poor and unstable flame retardant effects of alloy wires and cables; addresses the impact of hydrogen and harmful impurities on product quality during production, reduces the burning loss value during casting, ensures the cleanliness of inclusions in the melt, and improves the quality of the wire; and solves the problems of low mechanical properties, conductivity, and stability of alloy wires.
[0006] The objective of this invention can be achieved through the following technical solutions:
[0007] An alloy wire includes a core of multiple strands of metal wire twisted together and an insulation layer wrapping the core. The insulation layer comprises the following raw materials in parts by weight: 95-105 parts polyethylene resin, 5-10 parts flame retardant, 0.02-0.1 parts dicumyl peroxide, 20-30 parts talc, 15-25 parts calcium carbonate, 10-20 parts carbon black, 4-6 parts polyethylene wax, 3-5 parts zinc oxide, 1-3 parts light stabilizer, and 2-4 parts antioxidant.
[0008] The flame retardant is prepared through the following steps:
[0009] S1. Phenylacetyltrimethoxysilane, 3-buten-1-ol, toluene, and tetraisopropyl titanate were added to a three-necked flask and reacted at 90°C for 24 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed twice with tartaric acid and then three times with sodium bicarbonate solution. The organic phase was dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure to obtain intermediate 1. The molar ratio of phenyltrimethoxysilane, 3-buten-1-ol, toluene, and tetraisopropyl titanate was 19 mL: 17 mL: 80 mL: 0.093 g.
[0010] When the molar ratio of phenyltrimethoxysilane to glycidol is controlled at 1:2, phenyltrimethoxysilane and glycidol will undergo the following chemical reaction under the catalysis of tetraisopropyl titanate, and the reaction process is shown below:
[0011]
[0012] S2. 1,4-Butanediol, intermediate 1, toluene, and tetraisopropyl titanate were added to a three-necked flask and reacted at 100°C for 36 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed twice with tartaric acid and then three times with sodium bicarbonate solution. The organic phase was dried over anhydrous magnesium sulfate, filtered, purified by vacuum distillation and column chromatography (using a mixed solvent of cyclohexane and ethyl acetate as the eluent, with a volume ratio of 1:1). Vacuum distillation was then performed to obtain intermediate 2. The molar ratio of 1,4-butanediol, intermediate 1, toluene, and tetraisopropyl titanate was 7.5 mL: 22.3 g: 100 mL: 0.075 g.
[0013] 1,4-Butanediol and intermediate 1 undergo the following chemical reaction under the catalysis of tetraisopropyl titanate, as shown in the following process:
[0014]
[0015] S3. After stirring hexachlorotriphosphazene and tetrahydrofuran evenly, a reaction solution was obtained and set aside. Then, under a nitrogen atmosphere at room temperature, 70wt% NaH, intermediate 2 and tetrahydrofuran were added to a three-necked flask and stirred evenly. The reaction solution was then slowly added to the three-necked flask, and the temperature was raised to 65℃ for 48 hours. After the reaction was completed, the mixture was cooled to room temperature, rotary evaporated, and finally recrystallized with ethyl acetate to obtain the flame retardant. The ratio of hexachlorotriphosphazene, intermediate 2 and NaH was 3.5g:21g:0.24g.
[0016] The three chlorine atoms of hexachlorotriphosphazene are active chlorines, which can undergo a substitution reaction with the -Cl group of intermediate 2 under the action of NaH to obtain a flame retardant. The reaction process is shown below:
[0017]
[0018] The flame retardant of this invention contains commonly used halogen-free flame retardant elements nitrogen, phosphorus, and silicon. Phosphorus can capture free radicals in the flame in the gas phase to prevent the spread of the combustion flame, and it can also catalyze the char formation reaction of the matrix, forming a dense phosphorus-containing char layer on the matrix surface, isolating the flame from heat transfer. The non-combustible gas formed by nitrogen can act as a gas source to extinguish the flame. When nitrogen and phosphorus are present simultaneously, the char layer formed by combustion expands and foams, forming a porous foam structure. This expanded, porous foam char layer blocks the process of heat and oxygen exchange between the material and the outside environment, thereby preventing combustion and improving flame retardant performance. The silicon-based flame retardant provides thermal stability. It exhibits excellent properties, capable of transforming into silicon dioxide at high temperatures, which strengthens the carbon layer on the matrix surface, further blocking flames and enhancing the flame retardant effect. The flame retardant molecule of this invention has a dendritic structure, with each "tree" containing a carbon-carbon double bond at its end. Under the action of a trace initiator, the carbon-carbon double bonds can chemically react with the carbon-carbon double bonds at the ends of the matrix resin. This ensures that the flame retardant is firmly bound to the matrix resin, making it difficult to migrate or fall off, thus providing a long-term and stable excellent flame retardant effect. On the other hand, it also promotes the cross-linking of polyethylene. The formation of cross-linked polyethylene with a three-dimensional network structure can improve the mechanical properties, corrosion resistance, and weather resistance of the insulation layer.
[0019] Furthermore, the wire core is prepared by the following steps:
[0020] Aluminum is added to a melting furnace and melted at 780℃. When the aluminum liquid appears, an aluminum silicate covering agent is added. After all the aluminum is melted, the temperature is maintained for 0.5 hours to obtain aluminum liquid. The aluminum silicate covering agent on the surface of the aluminum liquid is removed, and iron, magnesium, copper, boron, zirconium, lanthanum, cerium and aluminum silicate covering agent are added. The mixture is stirred evenly and maintained for 0.5 hours to obtain aluminum alloy liquid.
[0021] The temperature was then lowered to 735℃, the covering agent was removed, and refining agents KCl, MgCl2, and CaF2 were added for 0.5 hours of refining. The temperature was then maintained at 735℃ for rotary blowing degassing. After degassing, the temperature was lowered to 720℃, slag was removed, and the mixture was held at that temperature for 0.4 hours. A portion of the molten aluminum alloy was then subjected to rapid pre-furnace composition analysis using a spectrometer to ensure that the elemental composition of the molten aluminum alloy met the following requirements: iron 0.10-0.80%, magnesium 0.005-0.20%, copper 0.01-0.30%, boron 0.005-0.02%, zirconium 0.01-0.10%, lanthanum 0.01-0.10%, cerium 0.01-0.15%, with the balance being aluminum and some unavoidable impurities.
[0022] The aluminum alloy liquid with the required composition is taken out of the furnace and continuously cast and rolled to obtain an aluminum alloy rod. Then, the aluminum alloy rod is annealed at 320℃ for 12 hours. Subsequently, the aluminum alloy rod is drawn into an aluminum alloy wire using a wire drawing machine. Finally, the aluminum alloy wire is annealed at 320℃ for 0.5 hours to obtain an aluminum alloy wire. Multiple strands of aluminum alloy wire are twisted together to obtain the wire core.
[0023] A certain amount of iron can achieve solid solution strengthening, and iron has little effect on the electrical conductivity of aluminum; a certain amount of copper can reduce the amount of iron added and improve the processing performance of the alloy, thus playing a solid solution strengthening role; a certain amount of boron refines the casting structure and weld structure, reduces the tendency of the alloy to crack, and thus improves the mechanical and processing properties of the aluminum alloy; the addition of lanthanum and cerium partially eliminates the harmful effects of impurities such as iron and silicon on the alloy properties, and can also react with aluminum to form compounds such as LaAl4 and CeAl4 that are not easily decomposed at high temperatures, which greatly improves the heat resistance and stability of the wire core at high temperatures; the addition of Trace amounts of zirconium can precipitate fine Al3Zr particles, which are dispersed throughout the aluminum matrix, significantly inhibiting the recovery, recrystallization, and grain growth processes during heating, thus raising the recrystallization temperature of aluminum by about 100K. The addition of iron, magnesium, copper, boron, and rare earth elements to the wire core greatly improves its heat resistance, stability, mechanical properties, and electrical conductivity. The combination of rotary jet degassing and refining agents effectively refines molten aluminum, offering advantages such as good refining effect, no pollution, low loss, low refining gas consumption, and low aluminum dross content. The synergistic effect of these two refining methods improves product quality.
[0024] A method for preparing an alloy wire includes the following steps: using an extrusion process to wrap an insulation layer around the outer surface of the wire core, thereby obtaining the alloy wire.
[0025] The beneficial effects of this invention are as follows: the synergistic flame retardancy of nitrogen, phosphorus, and silicon improves the flame retardant performance of the alloy wire material; the chemical interaction between the carbon-carbon double bonds and the matrix resin ensures the excellent and stable flame retardant effect of the alloy wire material, while also promoting the formation of cross-linked polyethylene, thereby improving the mechanical properties, corrosion resistance, and weather resistance of the alloy wire material; the addition of elements such as iron, copper, magnesium, boron, and rare earth elements improves the stability, mechanical properties, and electrical conductivity of the alloy wire; the combination of rotary jet degassing and refining agent reduces the burn-off value, ensuring the product quality of the alloy wire; the synergistic effect of each component greatly enhances the overall performance of the alloy wire of this invention. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] Example 1
[0028] The specific steps for preparing aluminum alloy wire are as follows:
[0029] Aluminum is added to a melting furnace and melted at 780℃. When the aluminum liquid appears, an aluminum silicate covering agent is added. After all the aluminum is melted, the temperature is maintained for 0.5 hours to obtain aluminum liquid. The aluminum silicate covering agent on the surface of the aluminum liquid is removed, and iron, magnesium, copper, boron, zirconium, lanthanum, cerium and aluminum silicate covering agent are added. The mixture is stirred evenly and maintained for 0.5 hours to obtain aluminum alloy liquid.
[0030] The temperature was then lowered to 735℃, the covering agent was removed, and refining agents KCl, MgCl2, and CaF2 were added for 0.5 hours of refining. The temperature was then maintained at 735℃ for rotary blowing degassing. After degassing, the temperature was lowered to 720℃, slag was removed, and the mixture was held at that temperature for 0.4 hours. A portion of the molten aluminum alloy was then subjected to rapid pre-furnace composition analysis using a spectrometer to ensure that the elemental composition of the molten aluminum alloy met the following requirements: iron 0.10-0.80%, magnesium 0.005-0.20%, copper 0.01-0.30%, boron 0.005-0.02%, zirconium 0.01-0.10%, lanthanum 0.01-0.10%, cerium 0.01-0.15%, with the balance being aluminum and some unavoidable impurities.
[0031] The aluminum alloy liquid with the required composition is taken out of the furnace and continuously cast and rolled to obtain an aluminum alloy rod. Then, the aluminum alloy rod is annealed at 320℃ for 12 hours. Subsequently, the aluminum alloy rod is drawn into an aluminum alloy wire using a wire drawing machine. Finally, the aluminum alloy wire is annealed at 320℃ for 0.5 hours to obtain an aluminum alloy wire.
[0032] Example 2
[0033] The remaining steps remain unchanged. Multiple strands of aluminum alloy wire from Example 1 are twisted together to prepare the wire core.
[0034] Example 3
[0035] The specific steps for preparing flame retardants are as follows:
[0036] S1. 19 mL of phenyltrimethoxysilane, 17 mL of 3-buten-1-ol, 80 mL of toluene and 0.093 g of tetraisopropyl titanate were added to a 250 mL three-necked flask and reacted at 90 °C for 24 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed twice with 5 wt% tartaric acid and then three times with 5 wt% sodium bicarbonate solution. The organic phase was dried with anhydrous magnesium sulfate, filtered, and distilled under reduced pressure to obtain intermediate 1.
[0037] S2. 7.5 mL of 1,4-butanediol, 22.3 g of intermediate 1, 100 mL of toluene, and 0.075 g of tetraisopropyl titanate were added to a 250 mL three-necked flask and reacted at 100 °C for 36 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed twice with 5 wt% tartaric acid and then three times with 5 wt% sodium bicarbonate solution. The organic phase was dried with anhydrous magnesium sulfate, filtered, purified by vacuum distillation and column chromatography (using a mixed solvent of cyclohexane and ethyl acetate as the eluent, with a volume ratio of cyclohexane to ethyl acetate of 1:1). Vacuum distillation was then performed to obtain intermediate 2.
[0038] S3. After stirring 3.5g of hexachlorotriphosphazene and 20mL of tetrahydrofuran until homogeneous, a reaction solution was obtained and set aside. Then, under a nitrogen atmosphere at room temperature, 0.24g of 70wt% NaH, 21g of intermediate 2 and 100mL of tetrahydrofuran were added to a 250mL three-necked flask and stirred until homogeneous. The reaction solution was then slowly added to the three-necked flask, and the temperature was raised to 65℃ and reacted for 48h. After the reaction was completed, the mixture was cooled to room temperature, rotary evaporated, and finally recrystallized with ethyl acetate to obtain the flame retardant.
[0039] Example 4
[0040] The specific steps for preparing the insulating layer are as follows:
[0041] 95 parts of polyethylene resin, 5 parts of the flame retardant from Example 3, 0.02 parts of dicumyl peroxide, 20 parts of talc, 15 parts of calcium carbonate, 10 parts of carbon black, 4 parts of polyethylene wax, 3 parts of zinc oxide, 1 part of light stabilizer HPT, and 2 parts of Solvay Cyanox 2777 antioxidant were fed into a twin-screw extruder for melt blending, and then extruded to obtain an insulating layer.
[0042] Example 5
[0043] The specific steps for preparing the insulating layer are as follows:
[0044] 98 parts of polyethylene resin, 6 parts of the flame retardant from Example 3, 0.03 parts of dicumyl peroxide, 22 parts of talc, 17 parts of calcium carbonate, 12 parts of carbon black, 5 parts of polyethylene wax, 4 parts of zinc oxide, 2 parts of light stabilizer HPT, and 3 parts of Solvay Cyanox 2777 antioxidant were fed into a twin-screw extruder for melt blending, and then extruded to obtain an insulating layer.
[0045] Example 6
[0046] The specific steps for preparing the insulating layer are as follows:
[0047] 105 parts of polyethylene resin, 10 parts of the flame retardant from Example 3, 0.1 parts of dicumyl peroxide, 30 parts of talc, 25 parts of calcium carbonate, 20 parts of carbon black, 6 parts of polyethylene wax, 5 parts of zinc oxide, 3 parts of light stabilizer HPT, and 4 parts of Solvay Cyanox 2777 antioxidant were fed into a twin-screw extruder for melt blending, and then extruded to obtain an insulating layer.
[0048] Example 7
[0049] The outer surface of the wire core prepared in Example 2 is wrapped with the insulation layer prepared in Example 4 using an extrusion process to obtain an alloy wire.
[0050] Example 8
[0051] An alloy wire is obtained by wrapping the outer surface of the wire core prepared in Example 2 with the insulation layer prepared in Example 5 using an extrusion process.
[0052] Example 9
[0053] An alloy wire is obtained by wrapping the outer surface of the wire core prepared in Example 2 with the insulation layer prepared in Example 6 using an extrusion process.
[0054] Comparative Example 1
[0055] The remaining steps remain unchanged, except that the refining agent from Example 1 is removed to prepare aluminum alloy wire.
[0056] Comparative Example 2
[0057] The remaining steps remain unchanged, except that the rotary blowing degassing of Example 1 is removed to prepare aluminum alloy wire.
[0058] Comparative Example 3
[0059] The remaining steps remain unchanged, except that the flame retardant from Example 6 is removed to prepare an insulating layer.
[0060] Comparative Example 4
[0061] The remaining steps remain unchanged, except that the flame retardant in Example 6 is replaced with Doher-606 flame retardant from Daer Chemical Co., Ltd., to prepare the insulating layer.
[0062] The aluminum alloy wires prepared in Example 1 and Comparative Examples 1-2 were subjected to the following performance tests, and the test results are shown in Table 1 below:
[0063] Table 1 Performance Test Results of Aluminum Alloy Wire
[0064] project resistivity Ω·m conductivity IACS Tensile strength (MPa) elongation % Example 1 <![CDATA[2.711×10 -8 ]]> 64.2% 141 16.2 Comparative Example 1 <![CDATA[2.738×10 -8 ]]> 61.3% 133 14.4 Comparative Example 2 <![CDATA[2.735×10 -8 ]]> 61.4% 135 14.5
[0065] As can be seen from Table 1 above, the aluminum alloy wire prepared by the embodiments of the present invention has excellent conductivity, tensile strength and elongation at break. From the comparison of the data of Example 1 with Comparative Example 1 and Comparative Example 2 in the table, it can be seen that the refining agent and rotary blowing degassing work together to improve the quality of the aluminum alloy wire in all aspects.
[0066] The insulating layers prepared in Examples 4-6 and Comparative Examples 3-4 were tested for limiting oxygen index (LOI) according to GB / T2406.2-2009 "Determination of flammability of plastics by oxygen index method - Part 2: Room temperature test". The test results are shown in Table 2 below.
[0067] Table 2 Performance test results of the insulation layer
[0068] project Limiting Oxygen Index (LOI) / % Example 4 36 Example 5 37 Example 6 39 Comparative Example 3 21 Comparative Example 4 30
[0069] As can be seen from the data in Table 2, the insulating layers prepared in Examples 4-6 of the present invention have excellent flame retardant effects, which are far superior to those prepared by commercially available flame retardants.
[0070] The test results in Tables 1 and 2 show that the alloy wires prepared by this invention have excellent conductivity, mechanical properties and flame retardancy, and have great application significance in the wire and cable industry.
[0071] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0072] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
Claims
1. An alloy wire, characterized in that, The product comprises a core of multi-strand aluminum alloy wires twisted together and an insulation layer encasing the core. The insulation layer comprises the following raw materials in parts by weight: 95-105 parts polyethylene resin, 5-10 parts flame retardant, 0.02-0.1 parts dicumyl peroxide, 20-30 parts talc, 15-25 parts calcium carbonate, 10-20 parts carbon black, 4-6 parts polyethylene wax, 3-5 parts zinc oxide, 1-3 parts light stabilizer, and 2-4 parts antioxidant. The flame retardant is prepared through the following steps: S1. Phenylacetyltrimethoxysilane, 3-buten-1-ol, toluene and tetraisopropyl titanate were added to a flask and reacted at 90°C for 24 h. The reaction product was first washed with tartaric acid, then washed with sodium bicarbonate solution, dried, filtered, and distilled under reduced pressure to obtain intermediate 1. S2. Add 1,4-butanediol, intermediate 1, toluene and tetraisopropyl titanate to a flask and react at 100°C for 36 h. Wash the reaction product with tartaric acid and then with sodium bicarbonate solution. Dry, filter, purify by vacuum distillation, column chromatography and vacuum distillation to obtain intermediate 2. S3. After stirring hexachlorotriphosphazene and tetrahydrofuran evenly, a reaction solution was obtained and set aside. Then, 70wt% NaH, intermediate 2 and tetrahydrofuran were added to a flask at room temperature and under a nitrogen atmosphere and stirred evenly. The reaction solution was then added to the flask and reacted at 65℃ for 48h. The flame retardant was obtained by rotary evaporation and recrystallization with ethyl acetate. The wire core is prepared through the following steps: Aluminum is added to a melting furnace and melted at 780℃. When the aluminum liquid appears, an aluminum silicate covering agent is added. After all the aluminum is melted, the temperature is maintained for 0.5 hours to obtain aluminum liquid. The aluminum silicate covering agent on the surface of the aluminum liquid is removed, and iron, magnesium, copper, boron, zirconium, lanthanum, cerium and aluminum silicate covering agent are added. The mixture is stirred evenly and maintained for 0.5 hours to obtain aluminum alloy liquid. The temperature was then lowered to 735℃, the covering agent was removed, and refining agents KCl, MgCl2, and CaF2 were added for 0.5 hours of refining. The temperature was then maintained at 735℃ for rotary blowing degassing. After degassing, the temperature was lowered to 720℃, slag was removed, and the mixture was held at that temperature for 0.4 hours. A portion of the molten aluminum alloy was then subjected to rapid pre-furnace composition analysis to ensure that the elemental composition of the molten aluminum alloy met the following requirements: iron 0.10-0.80%, magnesium 0.005-0.20%, copper 0.01-0.30%, boron 0.005-0.02%, zirconium 0.01-0.10%, lanthanum 0.01-0.10%, cerium 0.01-0.15%, with the balance being aluminum and some unavoidable impurities. The aluminum alloy liquid with the required composition is taken out of the furnace and continuously cast and rolled to obtain an aluminum alloy rod. Then, the aluminum alloy rod is annealed at 320℃ for 12 hours. Subsequently, the aluminum alloy rod is drawn into an aluminum alloy wire using a wire drawing machine. Finally, the aluminum alloy wire is annealed at 320℃ for 0.5 hours to obtain an aluminum alloy wire. Multiple strands of aluminum alloy wire are twisted together to obtain the wire core.
2. The alloy wire according to claim 1, characterized in that, In step S1, the ratio of phenyltrimethoxysilane, 3-buten-1-ol, toluene, and tetraisopropyl titanate is 19 mL: 17 mL: 80 mL: 0.093 g.
3. The alloy wire according to claim 1, characterized in that, In step S2, the ratio of 1,4-butanediol, intermediate 1, toluene, and tetraisopropyl titanate is 7.5 mL: 22.3 g: 100 mL: 0.075 g.
4. The alloy wire according to claim 1, characterized in that, In step S3, the ratio of hexachlorotriphosphazene, intermediate 2, and NaH is 3.5g: 21g: 0.24g.
5. The method for preparing an alloy wire according to claim 1, characterized in that, Includes the following steps: An insulation layer is wrapped around the outer surface of the wire core using an extrusion process to produce an alloy wire.
Citation Information
Patent Citations
Anti-aging insulating flame-retardant power cable
CN115785591A
Flame retardant resin composition and electric wire / cable by using the same