Impact resistant pressure sensitive adhesive

By using a pressure-sensitive adhesive with a specific formulation of poly(meth)acrylate and synthetic rubber components, the problems of insufficient impact resistance, internal strength and chemical resistance in the prior art have been solved, and multiple performance improvements of pressure-sensitive adhesives in electronic devices have been achieved.

CN117730128BActive Publication Date: 2026-11-24TESA SE
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202280046337.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-28
Filing Date
2022-06-27
Publication Date
2026-11-24
Estimated Expiration
2042-06-27

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesives are difficult to simultaneously satisfy good impact resistance, internal strength, adhesive performance and chemical resistance in electronic devices, especially when they are exposed to amphiphilic substances.

Method used

Pressure-sensitive adhesives based on poly(meth)acrylate and synthetic rubber components with specific formulations, including at least 50% by weight of poly(meth)acrylate, 15-35% by weight of vinyl aromatic butadiene and vinyl aromatic isoprene block copolymers, and a compatible tackifier resin, wherein the weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is from 1.1:1 to 2.5:1.

Benefits of technology

This invention achieves excellent impact resistance, high internal strength, and chemical resistance of pressure-sensitive adhesives in electronic devices, especially chemical resistance to amphiphilic substances, thus meeting the miniaturization and performance requirements of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117730128B_ABST
    Figure CN117730128B_ABST
Patent Text Reader

Abstract

The aim is to provide pressure-sensitive adhesives with good impact resistance and high internal strength, particularly against loads in the z-direction. This is achieved using a pressure-sensitive adhesive comprising a) at least 50% by weight of at least one poly(meth)acrylate based on the total weight of the pressure-sensitive adhesive; b) 15-35% by weight of a synthetic rubber component based on the total weight of the pressure-sensitive adhesive, comprising at least one vinyl aromatic butadiene block copolymer and at least one vinyl aromatic isoprene block copolymer; and c) at least one tackifier resin compatible with the synthetic rubber component, characterized in that the weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is 1.1:1 to 2.5:1. Another subject of the invention is an adhesive tape comprising at least one layer of a pressure-sensitive adhesive according to the invention, and the use of the pressure-sensitive adhesive according to the invention and / or the adhesive tape according to the invention as an adhesive in the manufacture of electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to the technical field of pressure-sensitive adhesives, such as those used as pressure-sensitive adhesives themselves or as components of tapes in various industrial fields. In particular, this invention proposes impact-resistant (or shock-resistant) pressure-sensitive adhesives based on poly(meth)acrylate and specific synthetic rubber components with good cohesive strength. The pressure-sensitive adhesives of this invention are particularly suitable for manufacturing electronic devices.

[0002] In many technical fields, adhesive tapes are increasingly used for bonding components. More often, tapes must meet very different, often contradictory, requirements. For example, good adhesion is almost always required, but it is often combined with good cohesion. Adhesion is essentially based on the ability of the pressure-sensitive adhesive in the tape to flow over the adhered material. However, increasing cohesion usually requires increasing the viscosity of the pressure-sensitive adhesive, and thus reducing its flowability. From this illustrative example, one can infer that the effects of various components must be carefully balanced in the formulation of pressure-sensitive adhesives to achieve satisfactory overall results.

[0003] In this context, pressure-sensitive adhesives have long been formulated based on mixtures or blends of poly(meth)acrylates and one or more synthetic rubbers. In this way, for example, pressure-sensitive adhesives can be achieved that exhibit good adhesion not only—depending on the properties of the polyacrylate component—on substrates with relatively high surface energy, but also on substrates with medium or low surface energy, such as specific plastic surfaces or other varnishes.

[0004] There are many examples in the prior art of how to achieve specific properties of pressure-sensitive adhesives by specifically selecting poly(meth)acrylate and synthetic rubber components.

[0005] US 4107233A describes improving the adhesion and printability of styrene-butadiene copolymers (SBCs) by adding polyacrylates.

[0006] EP 0 349 216 A1 discloses a method for improving the low-temperature impact resistance of polyacrylate pressure-sensitive adhesives by adding SBC, wherein 95 to 65 parts of polyacrylate are blended with 5 to 35 parts of SBC.

[0007] EP 0 352 901 A1 relates to pressure-sensitive adhesives comprising 60 to 95 parts of UV-polymerized polyacrylate and 35 to 5 parts of synthetic rubber. This formulation improves low-temperature impact resistance and adhesion to paints.

[0008] EP 0 437 068 A2 discloses a honeycomb pressure-sensitive adhesive film with improved low-temperature impact resistance based on a polyacrylate / SBC blend.

[0009] WO 95 / 19393A1 describes blends of styrene block copolymers modified with carboxyl groups and polyacrylates containing at least one nitrogen-containing monomer type. One objective of this method is to improve adhesion to low-energy substrates.

[0010] WO 2008 / 070386A1 describes a polymer blend comprising at least 92 parts of an SBC-based adhesive and at most 10 parts of a polyacrylate component.

[0011] WO 2000 / 006637 A1 discloses a blend of polyacrylate and SBC as a base material for foamed adhesive layers.

[0012] EP 2 832 811 A1 discloses a pressure-sensitive adhesive intended to achieve good adhesive strength at both high and low temperatures. The pressure-sensitive adhesive comprises the following components:

[0013] 40-70% by weight of at least one poly(meth)acrylate,

[0014] 15-50% by weight of at least one synthetic rubber, and

[0015] At least one tackifier compatible with poly(meth)acrylate.

[0016] In the production of electronic devices, the use of tapes and pressure-sensitive adhesives is increasing due to the ongoing trend towards miniaturization. This allows for significantly more precise positioning and space-saving bonding between components. However, the growing global demand for communication and entertainment electronics, coupled with increasing demands for device performance, is constantly influencing the use of pressure-sensitive adhesives.

[0017] The object of this invention is to provide a pressure-sensitive adhesive that exhibits good impact resistance and high internal strength, particularly relative to stress (load) in the z-direction. Of course, the pressure-sensitive adhesive should also possess good adhesive properties.

[0018] Another object of the present invention is to design the specified pressure-sensitive adhesive in such a way that, in addition to the properties already mentioned, it also has good chemical resistance, particularly to amphiphilic substances.

[0019] The achievement of this objective is based on the concept of using a poly(meth)acrylate-based pressure-sensitive adhesive that incorporates a synthetic rubber component with a specific formulation.

[0020] The first and general subject of this invention is pressure-sensitive adhesives, comprising

[0021] a) At least 50% by weight of at least one poly(meth)acrylate based on the total weight of the pressure-sensitive adhesive;

[0022] b) A synthetic rubber component comprising 15-35% by weight of the total weight of the pressure-sensitive adhesive, comprising at least one vinyl aromatic butadiene block copolymer and at least one polyvinyl aromatic isoprene block copolymer; and

[0023] c) At least one tackifier resin compatible with the synthetic rubber component

[0024] It is characterized in that the weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is 1.1:1 to 2.5:1.

[0025] This pressure-sensitive adhesive can achieve the required performance profile.

[0026] As generally understood, pressure-sensitive adhesives are materials that maintain a durable bond with a substrate even under relatively mild contact pressure. Pressure-sensitive adhesives typically possess inherent, durable tack at room temperature, meaning they exhibit a certain degree of viscosity and contact tack. This is particularly due to the fact that they wet the surface of the substrate even under mild contact pressure.

[0027] Without wishing to be bound by this theory, it is often assumed that pressure-sensitive adhesives can be considered as highly viscous liquids of an elastic component (part), which accordingly possess viscoelastic properties characteristic of the aforementioned persistent inherent tack and pressure-sensitive adhesiveness. It is assumed that in the case of pressure-sensitive adhesives, both a viscous flow process and the formation of elastic restoring forces exist upon mechanical deformation. A proportional (in certain proportions) viscous flow is used to achieve adhesion, while a proportional elastic restoring force is particularly necessary to achieve cohesion. The correlation between rheology and contact tack is known in the prior art and is described, for example, in "Satas, Handbook of Pressure Sensitive Adhesives Technology," third edition (1999), pp. 153–203.

[0028] The magnitudes of the elastic and viscous components are typically characterized using storage modulus (G') and loss modulus (G”), which can be determined by dynamic mechanical analysis (DMA), for example using a rheometer, as disclosed in WO 2015 / 189232A1.

[0029] In the context of this invention, when at a temperature of 23°C, at 10 0 Up to 10 1 Within the deformation frequency range of rad / s, G' and G” are each at least partially within 103 Up to 10 7 When Pa is within a certain range, the adhesive is preferably considered as a pressure-sensitive adhesive, and therefore is considered as a pressure-sensitive adhesive.

[0030] Poly(meth)acrylates are well known to those skilled in the art. In the context of this invention, as understood by those skilled in the art, the term "poly(meth)acrylate" includes polyacrylates and polymethacrylates.

[0031] According to the present invention, the pressure-sensitive adhesive comprises at least 50% by weight of at least one poly(meth)acrylate. In principle, the pressure-sensitive adhesive may comprise (exactly) one poly(meth)acrylate or two or more poly(meth)acrylates. In the plural "multiple poly(meth)acrylates" used below, this explicitly includes embodiments having (exactly) one poly(meth)acrylate.

[0032] The pressure-sensitive adhesive of the present invention preferably comprises no more than 70% by weight, particularly 52% to 65% by weight, and most preferably 54% to 60% by weight of poly(meth)acrylate.

[0033] The glass transition temperature of the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention is preferably <10°C, more preferably <0°C, and particularly preferably between -5°C and -30°C. The glass transition temperature of the polymer blocks in the polymer or block copolymer is determined according to the present invention by dynamic scanning calorimetry (DSC). For this purpose, approximately 5 mg of untreated polymer sample is weighed into an aluminum crucible (volume 25 μL) and sealed with a perforated cap. For the measurement, a DSC 204F1 from Netzsch is used. The measurement is performed under nitrogen to inertize the sample. The sample is first cooled to -150°C, then heated to +150°C at a rate of 10 K / min, and then cooled again to -150°C. A subsequent second heating curve is run again at a rate of 10 K / min, and the change in heat capacity is recorded. The glass transition is considered as a step in the thermogram.

[0034] The glass transition temperature T is obtained as follows. g (see Figure 1 ):

[0035] The linear ranges of the measurement curves before and after the step extend in the direction of increasing (the region before the step) or decreasing (the region after the step) temperature (tangents ① and ②). In the region of the step, the fitted line ⑤ is placed parallel to the vertical axis such that it intersects the two tangents, precisely forming two equal areas ③ and ④ (between the corresponding tangent, fitted line, and measurement curve). The intersection of the fitted line and the measurement curve in this location gives the glass transition temperature.

[0036] The poly(meth)acrylate in the pressure-sensitive adhesive of the present invention preferably comprises at least one partially polymerized functional monomer, more preferably reacting with an epoxy group to form a covalent bond. Most preferably, the partially polymerized functional monomer, more preferably reacting with an epoxy group to form a covalent bond, comprises at least one functional group selected from the group consisting of carboxylic acid, sulfonic acid, phosphonic acid, hydroxyl, anhydride, epoxy group, and amino; it particularly comprises at least one carboxylic acid group. Most preferably, the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention comprises partially polymerized acrylic acid and / or methacrylic acid. All mentioned groups are reactive with epoxy groups, which means that the poly(meth)acrylate is advantageously suitable for thermal crosslinking with the introduced epoxide.

[0037] The poly(meth)acrylate in the pressure-sensitive adhesive of the present invention is preferably obtained from the following monomer composition:

[0038] a) 30% to 75% by weight of at least one acrylate of formula (I):

[0039] CH2=CH-C(O)OR 1 (I)

[0040] Where R I It is a straight-chain or branched alkyl group having 1-10 carbon atoms;

[0041] b) 20% to 65% by weight of at least one acrylate of formula (II):

[0042] CH2=CH-C(O)OR 2 (II)

[0043] Where R 2 It is a phenoxyalkyl group;

[0044] c) From 0% to 40% by weight of at least one acrylate of formula (III):

[0045] CH2=C(O)OR 3 (III)

[0046] Where R 3 It is an alkyl diglycol group or an alkoxyalkyl group;

[0047] d) 0.5% to 10% by weight of at least one acrylate monomer of formula (IV):

[0048] CH2=CH-C(O)OR 4 (IV)

[0049] Where R 4 It consists of a hydrogen atom or a hydroxyalkyl group having 1-4 carbon atoms.

[0050] It has been found that this polyacrylate not only has good pressure-sensitive adhesion properties, but also high chemical stability, and is therefore very suitable as the base material for the pressure-sensitive adhesive of the present invention.

[0051] R in equation (I) 1 Preferably selected from methyl, n-butyl, and 2-ethylhexyl, more preferably selected from n-butyl and 2-ethylhexyl. Most preferably, R in formula (I) 1 It is n-butyl.

[0052] R in equation (II) 2 Preferably, the monomer is a phenoxyethyl group, particularly a 2-phenoxyethyl group. The monomer composition of the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention comprises 22 to 60% by weight of phenoxyethyl acrylate.

[0053] R in equation (III) 3 Preferably, the monomer is an ethyl diethylene glycol group or a methoxyethyl group. The monomer composition of the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention comprises 1 to 40% by weight of monomer c).

[0054] R in equation (IV) 4 Preferably, it is a hydrogen atom.

[0055] In one embodiment, the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention is derived from the following monomer composition: 30-55% by weight of n-butyl acrylate, 0-25% by weight of methyl acrylate, 0-40% by weight of ethylene glycol acrylate, 0-25% by weight of methoxyethyl acrylate, 20-55% by weight of phenoxyethyl acrylate and 1-5% by weight of acrylic acid.

[0056] More preferably, the poly(meth)acrylate in the pressure-sensitive adhesive of the present invention is derived from the following monomer composition: 40 to 50 wt% n-butyl acrylate, 15 to 25 wt% methyl acrylate, 20 to 40 wt% phenoxyethyl acrylate and 1 to 5 wt% acrylic acid.

[0057] If the pressure-sensitive adhesive of the present invention comprises two or more poly(meth)acrylates, it is preferred that all poly(meth)acrylates are derived from one of the above-mentioned monomer compositions.

[0058] Poly(meth)acrylates can, in principle, be prepared using any free radical or free radical-controlled polymerization, as well as combinations of different polymerization methods. Besides conventional free radical polymerization, these can also be, for example, ATRP, nitroxide (NOx) / TEMPO-controlled polymerization, or the RAFT process. Poly(meth)acrylates can be prepared by copolymerizing monomers using conventional polymerization initiators and optionally chain transfer agents, either in bulk, in emulsions, such as in water or liquid hydrocarbons, or in solution at conventional temperatures.

[0059] Poly(meth)acrylate is preferably prepared by copolymerizing monomers in a solvent, more preferably in a solvent having a boiling range of 50 to 150°C, especially 60 to 120°C, using 0.01 to 5% by weight, especially 0.1 to 2% by weight (based on the total weight of the monomers in their respective cases) of a polymerization initiator.

[0060] All conventional initiators are suitable in principle. Examples of free radical sources are peroxides, hydroperoxides, and azo compounds, such as benzoyl peroxide, cumene hydroperoxide, cyclohexanone peroxide, di-tert-butyl peroxide, cyclohexylsulfonylacetyl peroxide, diisopropyl percarbonate, tert-butyl peroctanoate, and benzimidol. Preferred free radical initiators are 2,2'-azobis(2-methylbutyronitrile) or 2,2'-azobis(2-methylpropionitrile) (2,2'-azobisisobutyronitrile).

[0061] Preferred solvents for the preparation of poly(meth)acrylates are: alcohols, such as methanol, ethanol, n-propanol and isopropanol, n-butanol and isobutanol, especially isopropanol and / or isobutanol; hydrocarbons, such as toluene, and gasoline (solvent oil, Benzine) having a boiling range of 60 to 120°C; ketones, especially acetone, methyl ethyl ketone, methyl isobutyl ketone; esters, such as ethyl acetate; and mixtures of the foregoing solvents. Particularly preferred solvents are mixtures containing isopropanol in an amount of 2 to 15% by weight, particularly 3 to 10% by weight, based on the solvent mixture used.

[0062] A concentration step is preferably performed after the manufacture (polymerization) of poly(meth)acrylate, and further processing of the poly(meth)acrylate, particularly blending with other components of the pressure-sensitive adhesive of the present invention, is substantially solvent-free. Polymer concentration can be carried out in the absence of crosslinking agents and accelerators. However, concentration can also be carried out in the presence of one of these compound classes prior to concentration, thereby allowing concentration to proceed in the presence of these substances.

[0063] After the concentration step, the polymer can be transferred to a compounding machine. Concentration and compounding can also optionally be carried out in the same reactor.

[0064] The weight-average molecular weight M of poly(meth)acrylatew Preferably, the concentration is in the range of 20,000 to 2,000,000 g / mol; most preferably, it is in the range of 100,000 to 1,500,000 g / mol; and particularly preferably, it is in the range of 150,000 to 1,000,000 g / mol. For this purpose, it is advantageous to polymerize in the presence of suitable chain transfer agents such as thiols, halogen compounds, and / or alcohols to establish the desired average molecular weight.

[0065] In this specification, the number-average molecular weight M n and weight average molecular weight M w The values ​​were determined by gel permeation chromatography (GPC). 100 μl of clarified filtered sample (sample concentration 4 g / L) was analyzed. The eluent used was tetrahydrofuran containing 0.1% (v / v) trifluoroacetic acid. Measurements were performed at 25 °C.

[0066] The preparative column used was a PSS-SDV type column, 5μm. 8.0mm*50mm (Here and below, the following order is used to describe: type, particle size, porosity, inner diameter*length; Type used: PSS-SDV, 5μm as well as and Separation was performed using a combination of columns (each 8.0 mm × 300 mm) from Polymer Standards Service; detected using a Shodex RI71 differential refractometer. The flow rate was 1.0 ml / min. Calibration was performed using the commercially available ReadyCal Kit Poly(styrene)high from PSP Polymer Standard Service GmbH, Mainz. The results were generalized to polymethyl methacrylate (PMMA) using Mark-Houwink parameters K and α, thus providing data in PMMA mass equivalents.

[0067] The K value of poly(meth)acrylate measured in toluene (1% solution, 21°C) is preferably 30 to 90, more preferably 40 to 70. The Fikentscher K value is a measure of the polymer's molecular weight and viscosity.

[0068] The principle of the method is based on the capillary-viscosity method for determining the relative viscosity of the solution. For this purpose, the test substance is dissolved in toluene by shaking for 30 minutes to obtain a 1% solution. The flow time is measured in a Vogel-Ossag viscometer at 25°C, and this is used to determine the relative viscosity of the sample solution relative to the pure solvent. The K value (K = 1000k) can be read from a table according to Fikentscher [PEHinkamp, ​​Polymer, 1967, 8, 381].

[0069] The poly(meth)acrylate in the pressure-sensitive adhesive of the present invention preferably has a polydispersity PD < 4 and therefore a relatively narrow molecular weight distribution. Despite the relatively low molecular weight, the adhesive based thereon exhibits particularly good shear strength after crosslinking. Furthermore, the relatively low polydispersity makes it easier to process from the melt, as the flow viscosity is lower compared to poly(meth)acrylates with a wider distribution and substantially the same application properties. Poly(meth)acrylates with a narrow distribution can advantageously be prepared by anionic polymerization or by controlled radical polymerization, the latter being particularly suitable. The corresponding poly(meth)acrylates can also be prepared via N-oxygen groups. In addition, atom transfer radical polymerization (ATRP) can advantageously be used to synthesize poly(meth)acrylates with a narrow distribution, preferably using monofunctional or bifunctional secondary or tertiary halides as initiators, and complexes of Cu, Ni, Fe, Pd, Pt, Ru, Os, Rh, Co, Ir, Ag, or Au are used to extract the halides. RAFT polymerization is also suitable.

[0070] The poly(meth)acrylates in the pressure-sensitive adhesives of the present invention are preferably already crosslinked. More preferably, they are thermally crosslinked through a linkage reaction between the functional groups present therein and specially added thermal crosslinking agents—particularly through addition or substitution reactions. All of the following thermal crosslinking agents can be used:

[0071] -It ensures a sufficiently long processing time so that no gelling occurs during processing operations, especially during extrusion operations.

[0072] Furthermore, it leads to rapid post-crosslinking of the polymer at temperatures below the processing temperature, particularly at room temperature, to achieve the desired level of crosslinking.

[0073] Thermal crosslinking can be carried out under much milder conditions than radiation-induced crosslinking, which can occasionally have destructive effects. However, in principle, in the context of this invention, crosslinking of poly(meth)acrylates can also be achieved by photochemical radiation alone or additionally, wherein desired or crosslinking-promoting substances, such as UV crosslinking agents, may optionally be added.

[0074] In the pressure-sensitive adhesive of the present invention, the poly(meth)acrylate is preferably crosslinked via an epoxide or via one or more epoxy-containing substances. The epoxy-containing substances are particularly polyfunctional epoxides, i.e., those having at least two epoxy groups; resulting accordingly in the indirect linkage of the poly(meth)acrylate units with functional groups. The epoxy-containing substances can be aromatic or aliphatic compounds.

[0075] Particularly suitable polyfunctional epoxides include: oligomers of epichlorohydrins; epoxy ethers of polyols (especially ethylene glycol, propylene glycol and butylene glycol, polyethylene glycol, thiodiglycol, glycerol, pentaerythritol, sorbitol, polyvinyl alcohol, polyallyl alcohol, etc.); and polyphenols (especially resorcinol, hydroquinone, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)methane, bis(4-hydroxy-3,5-dibromophenyl)methane, bis(4-hydroxy-3,5-difluorophenyl)methane, 1,1 - bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3-chlorophenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)diphenylmethane, bis(4-hydroxyphenyl)phenylmethane, bis(4-hydroxyphenyl)phenylmethane Epoxy ethers of 4'-methylphenylmethane, 1,1-bis(4-hydroxyphenyl)-2,2,2-trichloroethane, bis(4-hydroxyphenyl)-(4-chlorophenyl)methane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)cyclohexylmethane, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 4,4'-dihydroxydiphenylsulfone, and their hydroxyethyl ethers; phenol-formaldehyde condensation products such as phenol alcohol and phenolic resins; S-containing epoxides and N-containing cyclic oxides. Oxides, such as N,N-diglycidylaniline and N,N'-dimethyldiglycidyl-4,4-diaminodiphenylmethane; and epoxides prepared by conventional methods from monounsaturated or polyunsaturated carboxylic acid esters of unsaturated alcohols; glycidyl esters, and polyglycidyl esters (which can be obtained by polymerization or copolymerization of glycidyl esters of unsaturated acids or by other acidic compounds (e.g., from cyanuric acid, diglycidyl sulfide or cyclic trimethylenetrisulfone or derivatives thereof)).

[0076] Examples of very suitable ethers are butane-1,4-diol diglycidyl ether, polyglycerol-3-glycidyl ether, cyclohexanediethanol diglycidyl ether, glycerol triglycidyl ether, neopentyl glycol diglycidyl ether, pentaerythritol tetraglycidyl ether, hexane-1,6-diol diglycidyl ether, polypropylene glycol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, bisphenol A diglycidyl ether, and bisphenol F diglycidyl ether.

[0077] Another preferred epoxide is an alicyclic epoxide, such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexane carboxylate.

[0078] More preferably, the poly(meth)acrylate is crosslinked using a crosslinking agent-accelerator system (“crosslinking system”) to achieve better control over processing time, crosslinking kinetics, and degree of crosslinking. The crosslinking agent-accelerator system preferably comprises at least one epoxy group-containing substance as a crosslinking agent and at least one substance as an accelerator that promotes the crosslinking reaction of the epoxy group-containing compound at a temperature below the melting temperature of the polymer to be crosslinked.

[0079] The accelerators used according to the invention are more preferably amines. These should be considered, in a formal sense, as substituted products of ammonia; in the following formula, the substituents are represented by "R" and particularly include alkyl and / or aryl groups. Those amines that react with the polymer to be crosslinked at only a low level (if any) are particularly preferred.

[0080] In principle, the selected accelerator can be a primary amine (NRH2), a secondary amine (NR2H), or a tertiary amine (NR3), and of course, those having multiple primary and / or secondary and / or tertiary amine groups. Particularly preferred accelerators are tertiary amines, such as triethylamine, triethylenediamine, benzyldimethylamine, dimethylaminomethylphenol, 2,4,6-tris(N,N-dimethylaminomethyl)phenol, and N,N'-bis(3-(dimethylamino)propyl)urea. Other preferred accelerators are polyfunctional amines such as diamines, triamines, and / or tetraamines, for example, diethylenetriamine, triethylenetetramine, and trimethylhexamethylenediamine.

[0081] Another preferred accelerator is an amino alcohol. Secondary and / or tertiary amino alcohols are particularly preferred, wherein, in the case of two or more amine functional groups per molecule (functionality), at least one of the amine functional groups is preferably secondary and / or tertiary. Particularly preferred accelerators of this type are triethanolamine, N,N-bis(2-hydroxypropyl)ethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, 2-aminocyclohexanol, bis(2-hydroxycyclohexyl)methylamine, 2-(diisopropylamino)ethanol, 2-(dibutylamino)ethanol, N-butyldiethanolamine, N-butylethanolamine, 2-[bis(2-hydroxyethyl)amino]-2-(hydroxymethyl)-1,3-propanediol, 1-[bis(2-hydroxyethyl)amino]-2-propanol, triisopropanolamine, 2-(dimethylamino)ethanol, 2-(diethylamino)ethanol, 2-(2-dimethylaminoethoxy)ethanol, N,N,N'-trimethyl-N'-hydroxyethylbisaminoethyl ether, N,N,N'-trimethylaminoethylethanolamine, and N,N,N'-trimethylaminopropylethanolamine.

[0082] Other suitable accelerators include pyridine, imidazoles (e.g., 2-methylimidazolium), and 1,8-diazabicyclo[5.4.0]undec-7-ene. Alicyclic polyamines can also be used as accelerators. Suitable accelerators are also phosphorus-based, such as phosphine and / or... Compounds, such as triphenylphosphine or tetraphenylphosphine Tetraphenylborate.

[0083] Quaternary ammonium compounds can also be used as accelerators; examples are tetrabutylammonium hydroxide, hexadecyltrimethylammonium bromide, and benzalkonium chloride.

[0084] In addition to covalent crosslinking agents, such as, in particular, epoxides, isocyanates, and / or aziridines, preferred thermal crosslinking agents are also coordination crosslinking agents, especially metal chelates, particularly aluminum, titanium, zirconium, and / or iron chelates. Combinations of different crosslinking agents can also be used, such as combinations of one or more epoxides with one or more metal chelates.

[0085] A particularly preferred metal chelate is an aluminum chelate, such as aluminum acetylacetonate (III). These crosslinking agents are preferably used in amounts of 0.01 to 0.1 parts by weight, more preferably 0.02 to 0.08 parts by weight, based in their respective cases on 100 parts by weight of poly(meth)acrylate (solvent-free form).

[0086] Very particularly preferred thermal crosslinking agents are epoxides, especially those having tertiary amine functional groups, such as tetraglycidyl-m-phenylenediamine (N,N,N',N'-tetra(epoxyethylmethyl)-1,3-phenylenediamine). These compounds are preferably used in amounts of 0.03 to 0.1 parts by weight, more preferably 0.04 to 0.07 parts by weight, based in their respective cases on 100 parts by weight of polyacrylate (solvent-free form).

[0087] The pressure-sensitive adhesive of the present invention further includes at least one vinyl aromatic butadiene block copolymer and at least one polyvinyl aromatic isoprene block copolymer. Each may comprise (a single) vinyl aromatic butadiene block copolymer and vinyl aromatic isoprene block copolymer, but may also independently comprise two or more vinyl aromatic butadiene block copolymers and vinyl aromatic isoprene block copolymers. The pressure-sensitive adhesive of the present invention preferably comprises a total of 20% to 30% by weight of vinyl aromatic butadiene block copolymers and vinyl aromatic isoprene block copolymers, based on the total weight of the pressure-sensitive adhesive. The plural form "multiple vinyl aromatic butadiene block copolymers and multiple vinyl aromatic isoprene block copolymers" explicitly also includes cases where the pressure-sensitive adhesive of the present invention comprises only one vinyl aromatic butadiene block copolymer and / or vinyl aromatic isoprene block copolymer in each case.

[0088] Block copolymers of vinyl aromatic compounds and conjugated dienes are known in principle to those skilled in the art. The vinyl aromatic butadiene block copolymers and vinyl aromatic isoprene block copolymers in the pressure-sensitive adhesives of the present invention can substantially have AB, ABA, or (AB) compositions. n (AB) n X or (ABA) n X-form structure

[0089] in

[0090] -A blocks are each independently a vinyl aromatic block;

[0091] -B blocks are each independently a polybutadiene or polyisoprene block;

[0092] -X represents a residue (group) of the coupling agent or initiator, and

[0093] -n is an integer ≥2.

[0094] The pressure-sensitive adhesive of the present invention may also contain a mixture of different vinyl aromatic block copolymers having the above-described structure.

[0095] The vinyl aromatic block copolymer of the synthetic rubber component in the pressure-sensitive adhesive of the present invention therefore comprises one or more rubbery blocks B (soft blocks) and one or more glassy blocks A (hard blocks). More preferably, at least one and most preferably two of the vinyl aromatic block copolymers in the pressure-sensitive adhesive of the present invention are block copolymers having an AB or ABA structure, wherein A and B have the above-described definitions.

[0096] Preferably, the vinyl aromatic isoprene block copolymer is correspondingly a linear block copolymer; equally preferably, the vinyl aromatic butadiene block copolymer is a linear block copolymer; more preferably, both the vinyl aromatic butadiene block copolymer and the vinyl aromatic isoprene block copolymer are linear block copolymers. Linear block copolymers have been found to be advantageous for the adhesive properties of the pressure-sensitive adhesives of the present invention.

[0097] The vinyl aromatic butadiene block copolymer preferably has a vinyl aromatic compound content of at least 25%, more preferably at least 28%, and particularly at least 30%. Based on findings obtained in the context of this invention, this has a favorable effect on the internal strength (cohesion) of the pressure-sensitive adhesive.

[0098] Conversely, vinyl aromatic isoprene block copolymers preferably have a vinyl aromatic compound content of no more than 25%, more preferably no more than 17%. This has been found to be particularly advantageous for the impact resistance of pressure-sensitive adhesives.

[0099] In one embodiment, the vinyl aromatic isoprene block copolymer is a radial block copolymer having a vinyl aromatic compound content of no more than 25%, particularly no more than 20%. Such block copolymers have been found to be advantageous in terms of adhesive strength and internal strength.

[0100] The vinyl aromatic isoprene block copolymer preferably has a diblock content of >50%, more preferably >65%, and particularly >75%. Similarly, the vinyl aromatic butadiene block copolymer preferably has a diblock content of >50%, more preferably >65%, and particularly >75%. It has been found that a high diblock content, particularly a high diblock content in the vinyl aromatic butadiene copolymer, is beneficial to the adhesive properties of the pressure-sensitive adhesive. More preferably, the diblock content of both the vinyl aromatic isoprene block copolymer and the vinyl aromatic butadiene block copolymer is greater than 50%, more preferably greater than 65%, and particularly greater than 75%.

[0101] In the pressure-sensitive adhesive of the present invention, the vinyl aromatic compound in the vinyl aromatic block copolymer of the synthetic rubber component is preferably styrene; preferably, the vinyl aromatic blocks of the vinyl aromatic block copolymer are correspondingly polystyrene blocks. Preferably, the vinyl aromatic butadiene block copolymer is therefore a styrene-butadiene block polymer, and the vinyl aromatic isoprene block copolymer is a styrene-isoprene block polymer. In particular, the vinyl aromatic butadiene block copolymer is a styrene-butadiene-styrene block copolymer (SBS), and the vinyl aromatic isoprene block copolymer is a styrene-isoprene-styrene block copolymer (SIS).

[0102] As previously described, in the pressure-sensitive adhesive of the present invention, poly(meth)acrylate or all poly(meth)acrylate typically exists in the form of a matrix or continuous phase, wherein a vinyl aromatic block copolymer is embedded as a dispersed phase. Therefore, the synthetic rubber component is also referred to hereinafter as the synthetic rubber phase. The synthetic rubber phase can exist in different forms within the poly(meth)acrylate matrix.

[0103] The mixture of poly(meth)acrylate and two or more vinyl aromatic block copolymers is therefore preferably homogeneous. The poly(meth)acrylate and vinyl aromatic block copolymers present in the pressure-sensitive adhesive are preferably immiscible at 23°C to achieve homogeneity. Therefore, the pressure-sensitive adhesive of the present invention preferably has at least a biphasic morphology, at least under a microscope and at least at room temperature. More preferably, the poly(meth)acrylate and vinyl aromatic block copolymers are non-uniformly miscible with each other in a temperature range of 0°C to 50°C, particularly -30°C to 80°C, so that the pressure-sensitive adhesive is in a biphasic form under a microscope at least within these temperature ranges.

[0104] If, even after thorough mixing, the formation of at least two physically and / or chemically stable phases can be detected under a microscope, one phase being rich in one component and the second phase being rich in another component, then the components are defined in the context of this specification as "non-homogeneous miscibility". The presence of a component in a negligible amount in another component, which does not prevent the formation of multiphase, is considered irrelevant here.

[0105] An example of a suitable analytical system for phase separation is a scanning electron microscope. However, phase separation can also be identified by the fact that, for example, in dynamic differential calorimetry (DSC), different phases have two independent glass transition temperatures. Phase separation exists according to the invention when it can be clearly demonstrated by at least one analytical method.

[0106] In the domain rich in synthetic rubber, additional multiphase nature can exist as a fine structure, in which vinyl aromatic blocks form one phase and isoprene and / or butadiene blocks form a second phase.

[0107] The weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is preferably 1.3:1 to 2.3:1, more preferably 1.5:1 to 2.1:1. With these weight ratios, particularly good internal strength and particularly high impact resistance in the z-direction are observed.

[0108] In addition to the components described in detail herein, the pressure-sensitive adhesive of the present invention preferably includes at least one tackifier resin (or adhesive resin). Tackifier resins and their role in pressure-sensitive adhesives are generally known to those skilled in the art; they are commonly referred to as tackifiers or adhesive strength enhancers. According to the general understanding of those skilled in the art, a "tackifier resin" is an oligomer or polymer resin that improves the self-adhesion (tackiness, inherent adhesion) of the pressure-sensitive adhesive compared to a otherwise identical pressure-sensitive adhesive without any tackifier.

[0109] The tackifier resin of the pressure-sensitive adhesive of the present invention is compatible with the synthetic rubber phase. This means that, compared to a pure mixture of synthetic rubber, the tackifier resin alters the glass transition temperature of the system obtained after complete mixing of the synthetic rubber and the tackifier resin, where even a mixture of synthetic rubber and the tackifier resin can only allocate one glass transition temperature. Incompatible tackifier resins will result in two glass transition temperatures, one of which can be allocated to the synthetic rubber mixture, and the other to the resin domain. In this respect, the glass transition temperature is determined by calorimetry using DSC (differential scanning calorimetry), as described herein.

[0110] The tackifier resin is preferably a hydrocarbon resin; more preferably selected from hydrogenated polymers of dicyclopentadiene; non-hydrogenated or selectively, partially or completely hydrogenated hydrocarbon resins based on C5, C5 / C9 or C9 monomer streams; and polyterpene resins, particularly those based on α-pinene and / or β-pinene and / or δ-limonene. The hydrocarbon resin preferably has a DAP value of at least 0°C, very preferably at least 20°C, and / or preferably at least 40°C, particularly preferably at least 60°C. For information on determining the DAP and MMAP values, see C. Donker, PSTC Annual Technical Seminar, Proceedings, pp. 149-164, May 2001.

[0111] The tackifier resin is most preferably a polyterpene resin, especially a polyterpene resin based on α-pinene and / or β-pinene and / or δ-limonene.

[0112] The pressure-sensitive adhesive of the present invention preferably comprises 7% to 25% by weight of one or more tackifier resins, based on the total weight of the pressure-sensitive adhesive.

[0113] The tackifier resin in the pressure-sensitive adhesive of the present invention is preferably incompatible with poly(meth)acrylate.

[0114] However, in one embodiment, the pressure-sensitive adhesive of the present invention comprises a tackifier resin compatible with the synthetic rubber component and another tackifier resin compatible with poly(meth)acrylate. The tackifier resin compatible with poly(meth)acrylate is preferably a (meth)acrylate resin, which is preferably present in the pressure-sensitive adhesive in a total amount of <10% by weight. Such addition improves adhesion to polar bonding substrates.

[0115] In one embodiment, the pressure-sensitive adhesive of the present invention has been foamed. Foaming can, in principle, be achieved by any desired chemical and / or physical method. However, the foamed pressure-sensitive adhesive of the present invention is preferably obtained by introducing microspheres and subsequently expanding them. "Microspheres" are understood to refer to hollow microbeads that are elastic and therefore expandable in their basic state and have a thermoplastic polymer shell. These beads are filled with a low-boiling-point liquid or liquefied gas. The shell material used is particularly polyacrylonitrile, PVDC, PVC, or polyacrylate. A suitable low-boiling-point liquid, especially a hydrocarbon of lower alkanes such as isobutane or isopentane, is encapsulated as a liquefied gas within the polymer shell under pressure.

[0116] The action of the microspheres, especially the thermal effect, causes the polymer shell to soften. Simultaneously, the liquid propellant present within the shell transforms into its gaseous state. Here, the microspheres irreversibly and in three dimensions expand. The expansion ends when the internal and external pressures reach equilibrium. Because the polymer shell is retained, a closed-cell foam is obtained.

[0117] When foaming via microspheres, the microspheres can be provided to the formulation as a batch, paste, or unmixed or mixed powder. The metering point of addition may be envisioned, for example, before or after the addition of poly(meth)acrylate, for example, as a powder together with synthetic rubber or as a paste at a later time point.

[0118] Many types of microspheres are commercially available, differing primarily in their size (diameter in the unexpanded state: 6 to 45 μm) and the onset temperature required for their expansion (75 to 220 °C). Unexpanded microsphere types can also be obtained as aqueous (aqueous) dispersions with a solids content or microsphere content of about 40 to 45 wt%, and additionally as polymer-bonded microspheres (masterbatches), for example, in ethylene vinyl acetate at a microsphere concentration of about 65 wt%. Both microsphere dispersions and masterbatches, such as DU products, are suitable for manufacturing the foamed pressure-sensitive adhesives of the present invention.

[0119] The foamed pressure-sensitive adhesive of the present invention can also be produced using so-called pre-expanded microspheres. In this group, expansion has already occurred before mixing into the polymer matrix. Pre-expanded microspheres are commercially available, for example, in... Name or DE (dry expansion) type name.

[0120] The density of the foamed pressure-sensitive adhesive of the present invention is preferably <1100 kg / m³. 3 More preferably <1000kg / m 3 More preferably, the density of the foamed pressure-sensitive adhesive of the present invention is 800 to 1000 kg / m³. 3 Especially 850 to 970 kg / m 3 .

[0121] According to the application areas and desired performance of the pressure-sensitive adhesives of the present invention, additional components and / or additives may be added thereto, either alone or in combination with one or more other additives or components, in their respective cases.

[0122] For example, the pressure-sensitive adhesive of the present invention may contain powdered and granular, particularly abrasive and reinforcing fillers, dyes and pigments, such as chalk (CaCO3), titanium dioxide, zinc oxide and / or carbon black.

[0123] Pressure-sensitive adhesives preferably contain one or more forms of chalk as fillers, more preferably Cretaceous (from) With a preferred proportion of up to 20% by weight, the adhesive properties (shear strength at room temperature, instantaneous bond strength to steel and PE) remain almost unchanged due to the addition of filler. Furthermore, a variety of organic fillers may be present.

[0124] Suitable additives for the pressure-sensitive adhesives used in this invention are also selected independently of other additives—non-expandable hollow polymer beads, solid polymer beads, hollow glass beads, solid glass beads, hollow ceramic beads, solid ceramic beads and / or solid carbon beads (“carbon microspheres”).

[0125] Furthermore, the pressure-sensitive adhesive of the present invention may include low flammability fillers, such as ammonium polyphosphate; conductive fillers, such as conductive carbon black, carbon fibers and / or silver-coated beads; thermally conductive materials, such as boron nitride, alumina, silicon carbide; ferromagnetic additives, such as iron (III) oxides; organic renewable raw materials such as wood flour, organic and / or inorganic nanoparticles, fibers; compounding agents, aging inhibitors, light stabilizers and / or anti-ozone agents.

[0126] Plasticizers may be present optionally. Measurable plasticizers may include, for example, (meth)acrylate oligomers, phthalates, cyclohexane dicarboxylate, water-soluble plasticizers, plasticizing resins, phosphates (esters), or polyphosphates (esters).

[0127] To adjust the thermal shear strength of pressure-sensitive adhesives, silica can be added, and it is advantageous to precipitate silica by surface modification with dimethyldichlorosilane.

[0128] A method for manufacturing the pressure-sensitive adhesive of the present invention may first include concentrating a polyacrylate solution or dispersion produced from a polymer product. Concentration of the polymer may be carried out in the absence of crosslinking agents and accelerators. However, no more than one of these substances may be added to the polymer prior to concentration, thereby allowing concentration to proceed in the presence of these substances.

[0129] Synthetic rubber and optionally one or more tackifier resins can be added to the mixture via a solid metering device. A side feeder can be used to introduce concentrated and optionally molten poly(meth)acrylate into the compounding machine. In certain embodiments of the method, concentration and compounding can also be carried out in the same reactor. The resin can also be fed at different locations in the process via a resin melting unit and additional side feeders, for example, after the introduction of synthetic rubber and poly(meth)acrylate.

[0130] Other additives and / or plasticizers may also be fed in solid or melt form, or in batches in combination with other formulation components.

[0131] Specifically, the compounding machine used can be an extruder. The polymers are preferably in molten form in the compounding machine because they have already been added in a molten state, or they will be heated to a molten state in the compounding machine. Advantageously, the polymer in the compounding machine is held in the melt by heating.

[0132] If accelerator substances are used for the crosslinking of poly(meth)acrylates, they are preferably added only shortly before further processing of the substantially prepared blend composition, particularly shortly before coating or molding in some other way. The time window for addition before coating depends particularly on the available working period, i.e., the processing time in the melt, without adversely altering the properties of the resulting product.

[0133] Crosslinking agents, such as epoxides, and accelerators may also be added shortly before further processing of the composition, i.e., advantageously in the phase described above for accelerators. For this purpose, it is advantageous when the crosslinking agent and accelerator are introduced into the process simultaneously at the same point, optionally as a mixture of epoxide and accelerator. In principle, the timing or location of addition of the crosslinking agent and accelerator can also be switched in the above implementation, such that the accelerator is added before the crosslinking agent.

[0134] The composition can be further processed after formulation, particularly when coated onto a permanent or temporary carrier. During use, the permanent carrier remains bonded to the adhesive layer, while the temporary carrier is removed in a later processing operation, such as during tape finishing, or shortly before or at the time of final application of the pressure-sensitive adhesive.

[0135] The self-adhesive composition can be applied using a hot melt coating nozzle known in principle to those skilled in the art, or preferably using a roll coating system (also known as a coating calender). The coating calender may advantageously consist of two, three, four or more rolls.

[0136] Preferably, at least one roller has an anti-stick roller surface. Preferably, all rollers of the calender that come into contact with the pressure-sensitive adhesive are configured to be anti-stick. The anti-stick roller surface used is preferably a steel-ceramic-silicone composite material. Such a roller surface is resistant to thermal and mechanical stresses.

[0137] It has been found that using roller surfaces with surface structures is particularly advantageous, especially in such a way that the surface does not form complete contact with the composition layer to be treated, but rather has a smaller contact area compared to a smooth roller. Structured rollers, such as metal engraving rollers, are particularly advantageous, for example, steel engraving rollers.

[0138] If the pressure-sensitive adhesive of the present invention is to be foamed, foaming can, in principle, be carried out in the mixing machine or after the composition is applied. To promote the processability of the pressure-sensitive adhesive composition, it is preferable to first manufacture the composition by a hot-melt method, for example as described above, and introduce a foaming agent, such as microspheres, during production, but only after it leaves the mixing machine is foamed or expanded. As already shown, a reduction in surface roughness can be achieved in this way, particularly for compositions foamed with microspheres. However, in this procedure, it is necessary to ensure that the composition or microspheres do not expand within the mixing machine. This can be achieved through appropriate pressure-temperature control in the mixing machine.

[0139] The present invention also provides an adhesive tape comprising at least one layer of the pressure-sensitive adhesive of the present invention. The pressure-sensitive adhesive of the present invention is particularly suitable for forming high layer thicknesses. Therefore, the thickness of the layer of the pressure-sensitive adhesive of the present invention is preferably 100 μm to 5000 μm, more preferably 150 μm to 3000 μm, particularly 200 μm to 2500 μm, for example 500 μm to 2000 μm.

[0140] The tape of the present invention preferably consists of layers of the pressure-sensitive adhesive of the present invention. This type of tape is known as a transfer tape. However, the pressure-sensitive adhesive may also exist as a carrier layer of a single-sided or double-sided tape, or form at least one pressure-sensitive adhesive outer layer of a single-sided or double-sided tape containing a carrier. Release pads typically applied to the pressure-sensitive adhesive for (temporary) protection are not considered part of the tape. Therefore, the tape of the present invention may consist solely of layers of the pressure-sensitive adhesive of the present invention, even if it is covered with a release pad.

[0141] The present invention also provides the use of the pressure-sensitive adhesive or tape of the present invention as an adhesive in the manufacture of electronic, optical or precision mechanical devices, particularly portable electronic, optical and precision mechanical devices.

[0142] This portable device is specifically designed for:

[0143] Cameras, digital cameras, video accessories (such as exposure meters, flashes, apertures, camera housings, lenses, etc.), film cameras, camcorders, minicomputers (mobile computers, handheld computers, handheld calculators), laptops, notebooks, netbooks, ultrabooks, tablets, handheld devices, electronic notebooks and managers (so-called "electronic managers" or "personal digital assistants", PDAs, handheld computers), modems;

[0144] Computer accessories and operating units for electronic devices, such as mice, drawing pads, drawing tablets, microphones, speakers, game consoles, joysticks, remote controls, remote controllers, and touchpads (touch pads);

[0145] Monitors, displays, screens, touchscreens (sensor screens, touchscreen devices), projectors;

[0146] E-book reading devices (“e-books”);

[0147] Mini TVs, pocket TVs, devices for playing movies, video players, radios (including mini radios and pocket radios), Walkmans, Discmans, music players (for CDs, DVDs, Blu-rays, cassettes, USB, MP3s, etc.), headphones, cordless phones, mobile phones, smartphones, walkie-talkies (two-way radios), hands-free phones, pagers (pagers, pagers);

[0148] Portable defibrillator, blood glucose meter, blood pressure monitor, pedometer, pulse meter;

[0149] Flashlight, laser pointer;

[0150] Motion detectors, optical amplifiers, binoculars, night vision equipment, GPS devices, navigation equipment, and portable interface devices for satellite communications;

[0151] Data storage devices (USB sticks, external hard drives, memory cards); and

[0152] Watches, digital watches, pocket watches, chain watches, stopwatches.

[0153] More specifically, the pressure-sensitive adhesive or tape of the present invention is used as an adhesive in the production of smartphones (mobile phones), tablet computers, laptops, cameras, camcorders, keyboards or touchpads. Example

[0154] Test methods

[0155] Test 1: Instantaneous adhesive strength to plastics

[0156] The adhesion strength to plastics was determined under test conditions of 23℃ + / -1℃ and 50% + / -5% relative humidity; the plastic substrate used was a PBT sheet reinforced with 30% glass fiber and having a surface roughness of 1μm.

[0157] For cleaning and conditioning purposes, the test sheet was first wiped with ethanol before measurement and then placed in air for 5 minutes to allow the solvent to evaporate. The side of the single-layer tape away from the test substrate was then covered with a 36 μm etched PET film to prevent stretching of the sample during measurement. The sample was then rolled onto the plastic substrate. For this, a 2 kg rubber roller was used to roll back and forth twice at a speed of 10 m / min. Immediately after rolling, the tape was torn off the plastic substrate at a 180° angle, and the force required for this was measured using a Zwick tensile tester. The measurement results are reported in N / cm and averaged from three individual measurements.

[0158] A bond strength of 5.5 N / cm or greater is considered a good result.

[0159] Test 2: Tension (static load) in the z-direction

[0160] The so-called static load test method is used to determine both the holding force and the deflection of the tape in the z-direction.

[0161] Cut a square frame-like sample (external dimensions 33mm x 33mm; edge width 2mm; internal dimensions (window cutout) 29mm x 29mm) from the tape to be inspected. Adhere this sample to an acetone-cleaned steel frame (external dimensions 45mm x 45mm; edge width 10mm; internal dimensions (window cutout) 25mm x 25mm). Adhere an acetone-cleaned steel window (external dimensions 35mm x 35mm) to the other side of the tape. The steel frame, tape frame, and steel window are bonded in such a way that their geometric centers and diagonals coincide (corner to diagonal). The bonding area is 248mm². 2 The adhesive was pressed at 248N for 5 seconds and stored at 23°C / 50% relative humidity for 72 hours.

[0162] On the side of the steel window opposite the adhesive component, a so-called T-block made of steel, with a base dimension of 20 x 20 mm, is applied over its entire area using suitable tape. The resulting specimen is suspended in a bracket with the T-block pointing downwards, where the specimen rests on the steel frame and the window frame, with the T-block correspondingly ground-down and not in contact with the bracket. The test is initiated by suspending a 1000g weight on the T-block. The deflection of the tape is then determined as the initial value. For this purpose, the distance between the outer side of the steel frame and the inner side of the window (i.e., the material thickness of the steel frame + adhesive component) at all four corners is measured using a slide ruler. This measurement is repeated after 2 hours, 5 hours, 24 hours, 48 ​​hours, 72 hours, 144 hours, and 196 hours.

[0163] In each case, the average of the four measurement points is used to determine the extent to which the deflection of the adhesive joint has changed and whether the adhesive joint is still intact.

[0164] The recorded results, in their respective cases, are both the holding time and the deflection of the three samples.

[0165] Good results showed a deflection of ≤0.02mm and a performance retention of >168h.

[0166] Test 3: DuPont test in the z-direction (impact resistance)

[0167] Cut a square frame sample (external dimensions 33mm x 33mm; edge width 2.0mm; internal dimensions (window cutout) 29mm x 29mm) from the tape to be inspected. Attach this sample to a PC frame (external dimensions 45mm x 45mm; edge width 10mm; internal dimensions (window cutout) 25mm x 25mm; thickness 3mm). Attach the 35mm x 35mm PC window to the other side of the double-sided tape. Adhere the PC frame, tape frame, and PC window together so that their geometric centers and diagonals overlap each other (corner to diagonal). The adhesive area is 248mm². 2 The bonded parts were subjected to 248N pressure for 5 seconds and stored at 23°C / 50% relative humidity for 24 hours.

[0168] Immediately after storage, the adhesive assembly consisting of the PC frame, tape, and PC window is clamped into the sample holder with the protruding edge of the PC frame, ensuring the assembly is horizontally oriented and the PC window is below the frame. The sample holder is then inserted centered into the support set on the "DuPont Impact Tester". Using a 190g punch, a circular impact geometry with a 20mm diameter is centered and flush against the window side of the PC window.

[0169] A 150g weight, guided on two guide rods, is dropped vertically from a height of 5cm onto an assembly consisting of a sample holder, a sample, and a punch arranged as follows (measurement conditions: 23°C, 50% relative humidity). The height of the dropped weight is increased in 5cm increments until the introduced impact energy, as a result of impact stress, damages the sample and the PC window separates from the PC frame.

[0170] To compare experiments using different samples, the energy was calculated as follows:

[0171] E[J] = Height[m] * Mass of the object[kg] * 9.81kg / m*s 2

[0172] Five samples were tested for each product, and the average energy value was reported as a characteristic number of impact resistance.

[0173] Test 4: Drop Test (Impact Resistance)

[0174] The drop tower test method, used for testing instrumented drop devices, is also used to measure impact resistance.

[0175] Cut a square frame sample (external dimensions 33mm x 33mm; edge width 2mm; internal dimensions (window cutout) 29mm x 29mm) from the tape (pressure-sensitive adhesive strip) to be inspected. Attach this sample to an acetone-cleaned steel frame (external dimensions 45mm x 45mm; edge width 10mm; internal dimensions (window cutout) 25mm x 25mm). Attach an acetone-cleaned steel window (external dimensions 35mm x 35mm) to the other side of the tape. Bond the steel frame, tape frame, and steel window so that their geometric centers and diagonals overlap each other (corner to diagonal). The bonding area is 248mm². 2 The bonded parts were subjected to 248N pressure for 5 seconds and stored at 23°C / 50% relative humidity for 24 hours.

[0176] Immediately after storage, the test specimen is placed on the sample holder of the instrumented drop device in such a manner that the assembly is horizontal with the steel window facing downwards. Measurements are taken automatically using an instrumented method with a 5 kg load and a 10 cm drop height. The kinetic energy introduced by the load breaks the adhesive bond by causing the tape between the window and the frame to break, with the force recorded every μs by a piezoelectric sensor. Therefore, the accompanying software provides a force-time graph after measurement, from which the maximum force F can be determined. 最大 Shortly before the rectangular impact geometry strikes the window, the velocity of the falling weight is determined by two gratings. Assuming the energy introduced is greater than the impact strength of the adhesive, the work done by the adhesive before complete separation—the separation work—is determined using the change in force, the time required for separation, and the velocity of the falling weight. Five test specimens are examined for each sample; the final result consists of the average of the separation work or maximum force of these five specimens.

[0177] Preparation of polyacrylate

[0178] A 300L reactor, typically used for free radical polymerization, was loaded with 47 kg of n-butyl acrylate, 20 kg of methyl acrylate, 30 kg of 2-phenoxyethyl acrylate, 3 kg of acrylic acid, and 72.4 kg of gasoline / acetone (70:30). After passing nitrogen through the reactor with stirring for 45 minutes, the reactor was heated to 58°C and 50 g of [unspecified substance] was added. 67(2,2'-azobis(2-methylbutyronitrile)). The jacket temperature was then raised to 75°C and the reaction was carried out at this constant external temperature. After a 1-hour reaction time, 10 g of [the mixture] was added. 67. Dilute with 20 kg gasoline / acetone (70:30) after 3 hours and with 10 kg gasoline / acetone (70:30) after 6 hours. To reduce residual initiator, add 0.15 kg at 5.5 hours and 7 hours respectively. 16 (di(4-tert-butylcyclohexyl) peroxide dicarbonate). The reaction was terminated after a 24-hour reaction time, and the product was cooled to room temperature. The solution was adjusted to a solid content of 38% by weight.

[0179] Preparation of pressure-sensitive adhesives

[0180] Example 1:

[0181] In a planetary roller extruder, synthetic rubber (names listed below, weight ratios see Table 1) is melted in granular form via a solid metering system. Subsequently, polyacrylate and polyterpene resins are concentrated and pre-melted in a single-screw extruder. A115, Microspheres 920DU40; Nouryon) and pigments ( N-FL) metered addition. Additional crosslinking agent (N-FL) added to the mixture. 1500). The melt is mixed and formed between two release films (silicified PET films) using a two-roll calender to obtain a layer with a thickness of 200 μm.

[0182] The resulting adhesive composition layer has the following composition: 57 wt% polyacrylate, 24 wt% synthetic rubber (according to the composition in Table 1), and 18 wt%... A115, 0.3% by weight of crosslinking agent, and 0.7% by weight of microspheres.

[0183] Synthetic rubber used:

[0184] SK1: 3520 (linear SIS, Zeon; 78% diblock content; 15% styrene content)

[0185] SK2: 1118 (Linear SBS, Kraton; 78% diblock content; 33% styrene content)

[0186] SK4: 3280 (linear SIS, Zeon; 17% diblock content; 25% styrene content)

[0187] SK5: Q SL 196 (linear SIS, Zeon; 58% diblock content, 18% styrene content)

[0188] Table 1: Composition and Results

[0189]

[0190]

[0191] ne - not according to the invention; A - adhesive breakage; fs - foaming breakage

Claims

1. Pressure-sensitive adhesives, including: a) At least 50% by weight of at least one poly(meth)acrylate based on the total weight of the pressure-sensitive adhesive; b) 15-35% by weight of a synthetic rubber component based on the total weight of the pressure-sensitive adhesive, comprising at least one vinyl aromatic butadiene block copolymer and at least one vinyl aromatic isoprene block copolymer; and c) At least one tackifier resin compatible with the synthetic rubber component; The product is characterized in that the weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is 1.1:1 to 2.5:

1.

2. The pressure sensitive adhesive according to claim 1, characterized in that The pressure-sensitive adhesive comprises up to 70% by weight of poly(meth)acrylate.

3. Pressure-sensitive adhesive according to one of claims 1 and 2, characterized in that The weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is 1.3:1 to 2.3:

1.

4. The pressure sensitive adhesive according to claim 1 or 2, characterized in that Both the vinyl aromatic butadiene block copolymer and the vinyl aromatic isoprene block copolymer are linear block copolymers.

5. The pressure sensitive adhesive according to claim 1 or 2, characterized in that The vinyl aromatic butadiene block copolymer has a vinyl aromatic compound content of at least 25%.

6. The pressure sensitive adhesive according to claim 1 or 2, characterized in that The vinyl aromatic isoprene block copolymer has a vinyl aromatic compound content of up to 20%.

7. The pressure sensitive adhesive according to claim 1 or 2, characterized in that The vinyl aromatic butadiene block copolymer is a styrene-butadiene block polymer and the vinyl aromatic isoprene block copolymer is a styrene-isoprene block polymer.

8. The pressure sensitive adhesive according to claim 1 or 2, characterized in that The tackifier resin is a polyterpene resin.

9. The pressure sensitive adhesive according to claim 1 or 2, characterized in that The pressure-sensitive adhesive is foamed.

10. The pressure sensitive adhesive according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive comprises 52% to 65% by weight of poly(meth)acrylate.

11. The pressure sensitive adhesive according to claim 10, characterized in that The pressure-sensitive adhesive comprises 54% to 60% by weight of poly(meth)acrylate.

12. The pressure sensitive adhesive according to claim 1 or 2, characterized in that, The glass transition temperature of the poly(meth)acrylate in the pressure-sensitive adhesive is <10°C.

13. The pressure-sensitive adhesive according to claim 12, characterized in that, The glass transition temperature of the poly(meth)acrylate in the pressure-sensitive adhesive is <0°C.

14. The pressure-sensitive adhesive according to claim 12, characterized in that, The glass transition temperature of the poly(meth)acrylate in the pressure-sensitive adhesive is between -5 and -30°C.

15. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The poly(meth)acrylate in the pressure-sensitive adhesive is derived from the following monomers: a) 30% to 75% by weight of at least one acrylate of formula (I): CH2=CH-C(O)OR 1 (I) wherein R I is a linear or branched alkyl group having 1-10 carbon atoms; b) 20% to 65% by weight of at least one acrylate of formula (II): CH2=CH-C(O)OR 2 (II) wherein R 2 is a phenoxyalkyl group; c) At least one acrylate of formula (III) from 0% to 40% by weight: CH2=C(O)OR 3 (III) wherein R 3 is an alkyl diglycol group or an alkoxyalkyl group; d) 0.5% to 10% by weight of at least one acrylate monomer of formula (IV): CH2=CH-C(O)OR 4 (IV) wherein R 4 is a hydrogen atom or a hydroxyalkyl group having 1-4 carbon atoms.

16. The pressure-sensitive adhesive according to claim 15, characterized in that, R in equation (I) 1 It is selected from methyl, n-butyl and 2-ethylhexyl.

17. The pressure-sensitive adhesive according to claim 15, characterized in that, R in formula (II) is a 2-phenoxyethyl group. 2 is a 2-phenoxyethyl group.

18. The pressure-sensitive adhesive according to claim 15, characterized in that, The monomer composition of the poly(meth)acrylate in the pressure-sensitive adhesive includes 22 to 60% by weight of phenoxyethyl acrylate.

19. The pressure-sensitive adhesive according to claim 15, characterized in that, R in formula (III) is an ethyl diglycol group or a methoxyethyl group. 3 R in formula (III) is an ethyl diglycol group or a methoxyethyl group.

20. The pressure-sensitive adhesive according to claim 15, characterized in that, R in formula (IV) is a hydrogen atom. 4 is a hydrogen atom.

21. The pressure-sensitive adhesive according to claim 15, characterized in that, The poly(meth)acrylate in the pressure-sensitive adhesive is derived from the following monomer composition: 30-55% by weight of n-butyl acrylate, 0-25% by weight of methyl acrylate, 0-40% by weight of ethylene glycol acrylate, 0-25% by weight of methoxyethyl acrylate, 20-55% by weight of phenoxyethyl acrylate and 1-5% by weight of acrylic acid.

22. The pressure-sensitive adhesive according to claim 15, characterized in that, The poly(meth)acrylate in the pressure-sensitive adhesive is derived from the following monomer composition: 40 to 50 wt% n-butyl acrylate, 15 to 25 wt% methyl acrylate, 20 to 40 wt% phenoxyethyl acrylate and 1 to 5 wt% acrylic acid.

23. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The weight average molecular weight M of the poly(meth)acrylate is in the range of 20 000 to 2 000 000 g / mol. w in the range of 20 000 to 2 000 000 g / mol.

24. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive comprises a total of 20% to 30% by weight of vinyl aromatic butadiene block copolymer and vinyl aromatic isoprene block copolymer, based on the total weight of the pressure-sensitive adhesive.

25. The pressure-sensitive adhesive according to claim 5, characterized in that, The vinyl aromatic butadiene block copolymer has a vinyl aromatic compound content of at least 28%.

26. The pressure-sensitive adhesive according to claim 5, characterized in that, The vinyl aromatic butadiene block copolymer has a vinyl aromatic compound content of at least 30%.

27. The pressure-sensitive adhesive according to claim 6, characterized in that, The vinyl aromatic isoprene block copolymer has a vinyl aromatic compound content of no more than 17%.

28. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The vinyl aromatic isoprene block copolymer is a radial block copolymer having a vinyl aromatic compound content of no more than 25%.

29. The pressure-sensitive adhesive according to claim 28, characterized in that, The vinyl aromatic isoprene block copolymer is a radial block copolymer having a vinyl aromatic compound content of no more than 20%.

30. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The vinyl aromatic isoprene block copolymer has a diblock content of >50%.

31. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The vinyl aromatic butadiene block copolymer has a diblock content of >50%.

32. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, Both the vinyl aromatic isoprene block copolymer and the vinyl aromatic butadiene block copolymer have a diblock content of more than 50%.

33. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The vinyl aromatic butadiene block copolymer is a styrene-butadiene-styrene block copolymer (SBS), and the vinyl aromatic isoprene block copolymer is a styrene-isoprene-styrene block copolymer (SIS).

34. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, Poly(meth)acrylate and vinyl aromatic block copolymers are non-miscible with each other in a temperature range of -30°C to 80°C.

35. The pressure-sensitive adhesive according to claim 3, characterized in that, The weight ratio of the vinyl aromatic butadiene block copolymer to the vinyl aromatic isoprene block copolymer is 1.5:1 to 2.1:

1.

36. The pressure-sensitive adhesive according to claim 8, characterized in that, The tackifier resin is a polyterpene resin based on α-pinene and / or β-pinene and / or δ-limonene.

37. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive comprises 7% to 25% by weight of one or more tackifier resins, based on the total weight of the pressure-sensitive adhesive.

38. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The tackifier resin in the pressure-sensitive adhesive is incompatible with poly(meth)acrylate.

39. The pressure-sensitive adhesive according to claim 1 or 2, characterized in that, The pressure-sensitive adhesive includes a tackifier resin compatible with synthetic rubber components and another tackifier resin compatible with poly(meth)acrylate.

40. The pressure-sensitive adhesive according to claim 9, characterized in that, Foamed pressure-sensitive adhesives are obtained by introducing microspheres and then expanding them.

41. The pressure-sensitive adhesive according to claim 9, characterized in that, The density of the foamed pressure sensitive adhesive is 800 to 1000 kg / m 3 .

42. A tape comprising at least one layer of a pressure-sensitive adhesive according to any one of claims 1 to 41.

43. Use of the pressure-sensitive adhesive according to any one of claims 1 to 41 and / or the tape according to claim 42 as an adhesive in the manufacture of electronic devices.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive tapes

    EP0352901A1

  • Cellular pressure-sensitive adhesive membrane

    EP0437068A2

  • Adhesive mass

    EP2832811A1

  • Block copolymer blend with certain acrylics