A gating system for a superalloy guide vane and applications

By designing a gating system for high-temperature alloy guide vanes, and adopting a bottom-pouring method and insulation cotton molding, the problems of uneven metal flow in the guide vane forming cavity and unfavorable temperature field distribution in the gating system were solved, achieving high yield and precision manufacturing.

CN117733111BActive Publication Date: 2026-11-24BEIJING XINGHANG MECHANICAL ELECTRICAL EQUIP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311804714.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-24
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

The uneven metal flow in the guide vane forming cavity and the unfavorable temperature field distribution in the gating system lead to numerous internal and surface defects in the castings and a low yield.

Method used

Design a casting system for high-temperature alloy guide vanes. The system adopts a bottom-pouring method. The gating system consists of a pouring cup, a main gating system, a runner, and an ingate. The connection between the ingate and the runner is designed with rounded corners. The insulation material is molded in segments and prepared by vacuum melting.

Benefits of technology

It achieves balanced metal flow, reduces internal and surface defects in castings, improves yield and dimensional accuracy, and meets the requirements of harsh aerospace environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117733111B_ABST
    Figure CN117733111B_ABST
Patent Text Reader

Abstract

This invention relates to a casting system and its application for high-temperature alloy guide vanes, belonging to the field of alloy manufacturing technology. It solves the problem of difficulty in controlling the temperature field and the flow balance of multiple ingates in existing technologies. The casting system for high-temperature alloy guide vanes includes a gating system and guide vane forming cavities located on both sides of the gating system, forming a two-piece structure. It adopts a bottom-pouring method: the connection between the horizontal gating and the ingate is designed with a radius of R1 rounded corner, 30mm≤R1≤80mm; the main gating uses W layers of insulation cotton, the sprue cup, horizontal gating, and ingate use Z layers of insulation cotton, and the first part of the guide vane forming cavity along the metal flow direction uses X layers of insulation cotton, and the second part uses Y layers of insulation cotton, satisfying Z=a*W, X=1.5*Y, where a is 1, 1.5, or 2. This invention ensures balanced flow in the ingate by designing a rounded corner R1 at the connection between the horizontal gating and the ingate; the use of synergistically layered insulation cotton in the casting system reduces guide vane defects and effectively improves dimensional accuracy and yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy manufacturing technology, and in particular to a casting system for high-temperature alloy guide vanes and its application. Background Technology

[0002] High-temperature alloys are a class of metallic materials that can operate for extended periods at temperatures above 600°C and under certain stress. They possess high high-temperature strength, excellent oxidation and corrosion resistance, and good fatigue performance and fracture toughness. Based on these characteristics, high-temperature alloys are important materials widely used in aviation, aerospace, petroleum, chemical, and shipbuilding industries.

[0003] Guide vanes (stationary vanes), as typical hot-end castings, often employ complex, thin-walled, multi-bladed integrated structures with significant variations in overall wall thickness. They operate under extreme temperatures, complex loads, and oxidizing atmospheres for extended periods, thus placing extremely high demands on both dimensional accuracy and the surface and internal quality of the castings. Due to turbulent metal flow during casting, the completion time of each casting varies, and heat dissipation from the pyrolysis areas is poor, resulting in complex cooling conditions and a yield rate below 30%.

[0004] The guide vanes of aero-engines and gas turbine components have a large overall profile, complex structure, and significant thickness variations, ranging from 0.9 mm to 26 mm at their thickest point. This makes complete mold filling difficult, and the castings often have numerous hot spots, leading to casting defects such as porosity, shrinkage cavities, and cracks, both internally and on the surface. Furthermore, ensuring dimensional accuracy is challenging. Therefore, designing a gating system to reduce internal and surface defects in the guide vanes and improve their dimensional accuracy and yield is a pressing problem that needs to be solved. Summary of the Invention

[0005] Based on the above analysis, the embodiments of the present invention aim to provide a gating system and application for high-temperature alloy guide vanes, to solve at least one of the following technical problems: 1. It is difficult to achieve a uniform metal flow rate in the multiple ingates opened on the guide vane forming cavity, making it impossible to guarantee the quality and yield of each guide vane; 2. The temperature field distribution of the gating is not conducive to the continuous sequential feeding of the pouring cup, main gating, runner, and ingate in sequence, and it is difficult to avoid the back feeding of the guide vane forming cavity to the ingate, which easily leads to defects such as insufficient filling, shrinkage cavities, cracks, and low dimensional accuracy; 3. The temperature field distribution of the guide vane forming cavity is not conducive to the sequential solidification of the guide vane and the effective feeding of the gating to the guide vane forming cavity, which easily leads to casting defects.

[0006] The objective of this invention is mainly achieved through the following technical solutions:

[0007] In a first aspect, embodiments of the present invention provide a casting system for a high-temperature alloy guide vane. The casting system includes a gating system and a guide vane forming cavity. The guide vane forming cavity is symmetrically arranged on both sides of the gating system, forming a two-piece structure, and employs a bottom-pouring method.

[0008] The gating system mainly consists of a sprue cup, a main gating system, a runner, and an ingate. The sprue cup is connected to the main gating system and is distributed vertically. The lower end of the main gating system is connected to the middle of the runner. M ingates are symmetrically arranged on the left and right sides of the runner. The connection between the ingate and the runner is designed with a rounded corner with a radius of R1, satisfying 30mm≤R1≤80mm. The vertical section of the gating system from the end of the ingate to the forming cavity of the guide vane is called the ingate.

[0009] The guide vane mainly consists of an upper edge plate, a blade body, and a lower edge plate. The lower edge plate includes N parallel thick-walled sections, each of which is equipped with an ingate.

[0010] Optionally, the main runner uses W layers of insulation cotton, and the pouring cup, runner and ingate all use Z layers of insulation cotton, satisfying: Z = a * W, where a represents the proportionality coefficient, and a takes at least one of 1, 1.5 or 2, and W is a natural number greater than or equal to 1.

[0011] Optionally, the guide vane forming cavity is defined as the first part and the second part along the direction of molten metal flow. The first part uses X layers of insulation cotton and the second part uses Y layers of insulation cotton, satisfying X = 1.5 * Y, where Y is a natural number greater than or equal to 1.

[0012] Optionally, the length ratio of the first part to the second part of the guide vane forming cavity in the vertical direction is 1:1.

[0013] Optionally, the number of thick-walled sections of the guide vanes and the number of ingates must satisfy: M=N≥4;

[0014] Where M is the number of ingates;

[0015] N represents the number of thick-walled sections of the guide vane.

[0016] Optionally, the ingate opened on the same guide vane forming cavity adopts a stepped design and is connected and matched with the thick-walled part of the guide vane.

[0017] Optionally, the insulation material may include at least one of asbestos, aluminum silicate, and calcium silicate.

[0018] Optionally, the guide vane may be made of at least one of nickel-based, titanium-based, or cobalt-based superalloys.

[0019] Secondly, the present invention also provides the application of the above-mentioned high-temperature alloy guide vane casting system, which is suitable for the casting process of complex thin-walled high-temperature alloys with parallel distributed thick-walled parts, and is particularly suitable for the production process of guide vanes.

[0020] Optionally, the guide vanes include at least one of single guide vanes, double guide vanes, triple guide vanes, and multi-stage guide vanes.

[0021] Furthermore, a vacuum melting and casting method was used to prepare high-temperature alloy guide vanes.

[0022] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0023] 1. The gating system for high-temperature alloy guide vanes provided by this invention includes a gating system and guide vane forming cavities. The guide vane forming cavities are symmetrically arranged on both sides of the gating system to form a two-piece structure. The bottom pouring method is adopted. The gating system mainly consists of a pouring cup, a main gating system, a horizontal gating system, and an inner gating system. The connection between the horizontal gating system and the inner gating system is designed with a rounded corner with a radius of R1, which satisfies 30mm≤R1≤80mm. This ensures that the metal flow rate entering each inner gating system through the horizontal gating system is basically consistent, thereby effectively controlling the metal flow rate entering each guide vane forming cavity to achieve balance, thus ensuring the internal and surface quality of each guide vane and the yield rate.

[0024] 2. In the casting system of the high-temperature alloy guide vane provided by the present invention, the guide vane is mainly composed of an upper edge plate, a blade body, and a lower edge plate. The lower edge plate includes N parallel thick-walled sections. An ingate is opened in the thick-walled section of the guide vane. On the one hand, it can ensure the flowability of the molten metal during mold filling. On the other hand, it is also conducive to the effective transmission of injection pressure and easier replenishment of material required when the liquid volume shrinks, thereby reducing the porosity and crack defects of the guide vane and improving the pass rate of the guide vane.

[0025] 3. In the casting system of the high-temperature alloy guide vane provided by the present invention, the number of N thick-walled parts and M ingates of the guide vane satisfies M=N≥4. The ingate is designed as a stepped type, which effectively ensures that the ingate provides sufficient feeding to the N thick-walled parts of the guide vane, thereby ensuring that the ingate provides sufficient feeding to the forming cavity of the guide vane, thus reducing the defects of loose shrinkage cavities in the high-temperature alloy guide vane and improving the quality of the high-temperature alloy guide vane.

[0026] 4. In the casting system for high-temperature alloy guide vanes provided by this invention, the gating system adopts an insulation cotton molding method: the main gating system is designed with W layers of insulation cotton, and the gating cup, horizontal gating system, and inner gating system are designed with Z layers of insulation cotton, satisfying: Z = a * W, where a represents a proportionality coefficient, and a takes at least one of 1, 1.5, or 2, and W is a natural number greater than or equal to 1. By utilizing the insulation cotton molding of the gating system and the synergistic effect between the layers of each part, it is effectively ensured that during the cooling process, the gating cup continuously feeds the main gating system, the main gating system effectively feeds the horizontal gating system, the horizontal gating system effectively feeds the inner gating system, and the inner gating system effectively feeds the guide vane forming cavity. This achieves sequential feeding of the gating system to the guide vane forming cavity, while ensuring that the gating system solidifies last without causing the guide vane forming cavity to feed the gating system back, effectively avoiding defects such as insufficient filling, shrinkage cavities, cracks, and low dimensional accuracy.

[0027] 5. In the casting system for high-temperature alloy guide vanes provided by the present invention, the guide vane forming cavity adopts a segmented insulation cotton design: the guide vane forming cavity is defined as a first part and a second part along the direction of molten metal flow. The first part adopts X layers of insulation cotton, and the second part adopts Y layers of insulation cotton, satisfying X = 1.5 * Y, where Y is a natural number greater than or equal to 1; more preferably, the length ratio of the first part and the second part of the guide vane forming cavity in the vertical direction is 1:1; the guide vane forming cavity adopts a segmented insulation cotton design: the first part and the second part are first designed with Y layers of insulation cotton as a whole to reduce the cooling rate, so that the cooling process of the guide vane is coordinated, forming directional solidification, reducing solidification stress, and reducing the tendency of guide vane deformation and cracking; furthermore, the first part is also added with 0.5Y layers of insulation cotton, which effectively ensures sufficient feeding of the guide vane forming cavity by the ingate, thereby ensuring the quality of the guide vane and a high yield.

[0028] 6. The application of the gating system for the above-mentioned high-temperature alloy guide vanes provided by this invention is suitable for the casting process of complex thin-walled high-temperature alloys with parallel thick-walled sections, and is particularly suitable for the production process of guide vanes. High-temperature alloy guide vanes have complex structures and large variations in wall thickness. Using the gating system provided by this invention to prepare guide vanes and similar structures can significantly reduce porosity and crack defects in the guide vanes, achieve precision manufacturing of high-temperature alloy guide vanes, and improve the yield and dimensional accuracy of the guide vanes.

[0029] 7. In practical applications, the casting system for the high-temperature alloy guide vane provided by the present invention uses a vacuum melting casting method to prepare the guide vane. Vacuum melting can achieve strict composition control, effectively remove gases and reduce non-metallic impurities, thereby improving the physical and mechanical properties of the high-temperature alloy guide vane and better meeting the harsh operating environment in aerospace.

[0030] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0031] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0032] Figure 1 This is a schematic diagram of the main structure of the casting system in an embodiment of the present invention;

[0033] Figure 2 This is a three-dimensional structural diagram of the casting system in an embodiment of the present invention;

[0034] Figure 3 for Figure 1 Schematic diagram of the horizontal runner and ingate in section B;

[0035] Figure 4 for Figure 1 Sectional view of AA;

[0036] Figure 5 for Figure 1 A three-dimensional structural diagram of the connection between the inlet runner and the guide vanes;

[0037] Figure 6 for Figure 1 A bottom view of the gating system.

[0038] Figure 7 for Figure 1 A bottom view of the lower edge plate of the guide vane;

[0039] Figure 8 The images show actual images of guide vanes prepared using the gating system described in Examples 1-3 of this invention.

[0040] Figure 9 Defect diagrams of guide vanes prepared using the gating systems of Comparative Examples 1-8;

[0041] Reference numerals: 1-Sprue cup; 2-Sprue; 3-Glide runner; 4-Ingate; 5-Guide blade; 6-Ingate; 7-Upper edge plate; 8-Blade; 9-Lower edge plate; 4a-First ingate; 4b-Second ingate; 4c-Third ingate; 4d-Fourth ingate; 6a-First ingate; 6b-Second ingate; 6c-Third ingate; 6d-Fourth ingate; S1-First stiffener; S2-Second stiffener; R1-Round radius of the corner at the connection between the horizontal section of the sprue and the ingate; R2-Round radius of the corner at the connection between the ingate and the horizontal section of the ingate. Detailed Implementation

[0042] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0043] Please see Figures 1 to 7 This invention provides a casting system for high-temperature alloy guide vanes, including a gating system and guide vane forming cavities. The guide vane forming cavities are symmetrically arranged on both sides of the gating system, and a bottom-pouring method is adopted. Preferably, but not limited to, a two-piece structure is used.

[0044] The gating system mainly consists of a pouring cup 1, a main gating system 2, a horizontal gating system 3, and an ingate system 4. The pouring cup 1 is connected to the main gating system 2 and is distributed vertically. The lower end of the main gating system 2 is connected to the middle of the horizontal gating system 3. M ingate systems are symmetrically arranged on the left and right sides of the horizontal gating system 3. Each ingate system is designed with a rounded corner with a radius of R1 at the connection with the horizontal gating system 3, satisfying 30mm≤R1≤80mm. This ensures that the metal flow into the M ingate systems is basically balanced, thereby ensuring the internal and surface quality of each guide vane and a high yield.

[0045] The shapes of the pouring cup 1 and the main runner 2 can vary depending on the specific circumstances; optionally, the pouring cup 1 is funnel-shaped or basin-shaped, and the main runner 2 is cylindrical or conical with a uniform cross-section.

[0046] The shape and positional relationship of the horizontal runner 3 and the ingate 4 can vary depending on the specific situation; optionally, the shape of the horizontal runner 3 is a cuboid; the shape of the horizontal section of the ingate 4 is a cuboid, but the connection with the horizontal runner 3 is designed with a rounded corner of radius R1, satisfying 30mm≤R1≤80mm; the angle between the liquid flow direction in the horizontal runner 3 and the liquid flow direction in the ingate 4 is greater than 90°, and more preferably, in this embodiment, the angle between the liquid flow direction in the horizontal runner 3 and the liquid flow direction in the M ingates is the same and is 120°.

[0047] Preferably, the bottoms of the horizontal runner 3 and the M ingates are flush.

[0048] It should be noted that, in this invention, the vertical runner between the end of the ingate 4 and the guide vane forming cavity is called the ingate 6; the shape of the ingate 6 can vary depending on the specific situation; in this embodiment, the longitudinal section of the ingate 6 is a trapezoid, with a base length of (60-95) mm and a height of (35-55) mm; the above example only shows one specific implementation of the ingate shape, and in practical applications, it includes, but is not limited to, this, and can be determined according to the specific situation, all of which are within the protection scope of this application.

[0049] Furthermore, the connection between the ingate 6 and the horizontal section of the ingate 4 is designed with a rounded transition of radius R2. The rounded corner R2 helps to reduce flow resistance and allows the molten metal to fill the cavity as quickly as possible. In this embodiment, R2 is 5 to 10 mm. The above example only shows one specific implementation of the connection between the ingate and the horizontal section of the ingate. In practical applications, there are other implementations, including but not limited to this one. No specific limitation is made here. It can be determined according to the specific situation and is within the protection scope of this application.

[0050] The guide vane 5 is mainly composed of an upper edge plate 7, a blade body 8, and a lower edge plate 9. The lower edge plate 9 includes N parallel thick-walled sections, each of which is provided with an ingate. The thickness of the ingate cross section is preferably, but not limited to, 50-80% of the thickness of the thick-walled section of the guide vane. On the one hand, this can ensure the flowability of the molten metal during mold filling. On the other hand, it is also conducive to the effective transmission of injection pressure and easier replenishment of material required when the liquid volume shrinks, thereby reducing the porosity and crack defects of the guide vane and improving the pass rate of the guide vane.

[0051] Preferably, the number of thick-walled sections of the guide vanes and the number of ingates satisfy the following conditions:

[0052] M = N ≥ 4;

[0053] Where M is the number of ingates;

[0054] N represents the number of thick-walled sections of the guide vane.

[0055] Optionally, in this embodiment, both M and N are 4.

[0056] Optional, such as Figure 6 As shown, the ingate 4 includes a first ingate 4a, a second ingate 4b, a third ingate 4c, and a fourth ingate 4d. The connection between the runner 3 and the four ingates is designed with a rounded corner with a radius of R1. Preferably, 30mm≤R1≤80mm. In this embodiment, the values ​​of R1 are 30mm, 50mm, and 80mm, respectively.

[0057] The thick-walled portion of the guide vane can vary depending on the specific circumstances; in this implementation, for example... Figure 4 , Figure 5 and Figure 7 As shown, the first stiffener S1 and the second stiffener S2 are two thick-walled portions of the guide vane. The end section of the first ingate 4a (i.e., the first ingate 6a) is connected to the first stiffener S1, and the end section of the second ingate 4b (i.e., the second ingate 6b) is connected to the second stiffener S2. The above example only shows one specific implementation of the thick-walled portion of the guide vane. In practical applications, it includes, but is not limited to, this example. It is not specifically limited here, but can be determined according to the specific circumstances, and all are within the protection scope of this application.

[0058] Preferably, the ingates formed on the same guide vane molding cavity are respectively connected and fitted with the thick-walled part of the guide vane, thereby forming a stepped ingate; in this embodiment, the first ingate 4a is connected and fitted with the first rib S1 through the first ingate 6a, and the second ingate 4b is connected and fitted with the second rib S2 through the second ingate 6b, thereby forming stepped ingates 4a and 4b, as shown. Figure 6 The third ingate 4c and the fourth ingate 4d are also connected to the two stiffeners of the guide vane on the other side in a stepped manner (not shown in the figure). The stepped design of the ingate effectively ensures that the ingate provides sufficient feeding to each thick-walled part of the guide vane, thereby reducing the defects of loose shrinkage cavities in the guide vane and improving the quality of the guide vane.

[0059] The material of the guide vane 5 can be selected according to actual needs, and may include, but is not limited to, at least one of high-temperature alloys such as nickel-based, titanium-based, and cobalt-based alloys.

[0060] The cross-sectional shape of the runner can be selected as needed. The pouring cup can be, but is not limited to, a funnel shape; the main runner can be, but is not limited to, a circle or a square shape; the runner can be, but is not limited to, a rectangle or a circle shape; and the ingate is generally a conformal structure to the structure of the guide vanes.

[0061] Furthermore, the gating system adopts a heat insulation cotton molding method. The main gating 2 uses W layers of heat insulation cotton, and the pouring cup 1, the horizontal gating 3 and the inner gating 4 all use Z layers of heat insulation cotton. The above number of layers satisfies: Z = a * W, where a represents a proportionality coefficient, and a takes at least one of 1, 1.5 or 2, and W is a natural number greater than or equal to 1; in this embodiment, W = 1.

[0062] By utilizing the insulation cotton design of the gating system and the synergistic effect between the layers of each part, it is effectively ensured that during the cooling process, the gating cup continuously replenishes the main gating system, the main gating system effectively replenishes the horizontal gating system, the horizontal gating system effectively replenishes the ingate system, and the ingate system effectively replenishes the guide vane forming cavity. This achieves sequential replenishment of the gating system to the guide vane forming cavity, while ensuring that the gating system solidifies last without causing the guide vane forming cavity to replenish the gating system in the opposite direction. This effectively avoids defects such as insufficient filling, shrinkage cavities, cracks, and low dimensional accuracy.

[0063] Preferably, the forming cavity of the guide vane 5 is defined as the first part and the second part along the upward flow direction of the molten metal, that is, the first part is close to the ingate and the second part is far away from the ingate; the first part uses X layers of insulation cotton and the second part uses Y layers of insulation cotton, satisfying X = 1.5 * Y, where Y is a natural number greater than or equal to 1; specifically, the insulation cotton is set on the periphery of the forming cavity of the guide vane.

[0064] More preferably, the length ratio of the first part to the second part of the forming cavity of the guide vane 5 in the vertical direction is 1:1.

[0065] The guide vane 5 forming cavity adopts a segmented insulation cotton design: the first part and the second part are designed with a Y-layer insulation cotton as a whole to reduce the cooling rate, so that the cooling process of the guide vane is coordinated, reducing solidification stress and reducing the tendency of guide vane deformation and cracking; furthermore, the first part is also added with a 0.5Y-layer insulation cotton, which effectively ensures sufficient feeding of the guide vane forming cavity by the ingate, thereby ensuring the quality of the guide vane and a high yield.

[0066] The material of the insulation cotton can be selected according to actual needs. Preferably, it includes at least one of asbestos, aluminum silicate, and calcium silicate; in this embodiment, the insulation cotton is aluminum silicate. Compared with the existing sand-filled molding or single-shell molding insulation methods, the insulation cotton molding has the advantages of simple operation, readily available raw materials, and easy industrialization.

[0067] The thickness of the insulation cotton can be selected according to the needs of the scale of the pouring system. For example, the thickness of each layer of insulation cotton can be 20mm. The above example only shows one specific implementation of the insulation cotton thickness. In actual applications, it is not limited to this. It can be determined according to the specific situation and is within the protection scope of this application.

[0068] The present invention also provides the application of the above-mentioned high-temperature alloy guide vane casting system, which is suitable for the casting process of complex thin-walled high-temperature alloys with parallel distributed thick-walled parts, and is particularly suitable for the production process of guide vanes.

[0069] Furthermore, the guide vanes include at least one of single guide vanes, double guide vanes, triple guide vanes, and multi-stage guide vanes.

[0070] In this embodiment, the guide vane is a double guide vane, mainly composed of an upper edge plate, a blade body, and a lower edge plate. The lower edge plate includes a first stiffener S1 and a second stiffener S2.

[0071] Preferably, the high-temperature alloy guide vane is prepared by vacuum melting and casting.

[0072] Example 1

[0073] like Figures 1 to 7 The gating system for the high-temperature alloy guide vanes in this embodiment includes a gating system and two guide vane forming cavities symmetrically arranged on both sides of the gating system, forming a two-piece structure, using a bottom-pouring method. The gating system mainly consists of a pouring cup 1, a main gating system 2, a horizontal gating system 3, and an ingate 4. The pouring cup 1 is funnel-shaped, the main gating system 2 has a circular cross-section, the pouring cup 1 is connected to the main gating system 2 and distributed vertically, the lower end of the main gating system 2 is connected to the middle of the horizontal gating system 3, the horizontal gating system 3 has a rectangular cross-section, and the horizontal gating system 3 is symmetrical on both sides. Four rectangular ingates are arranged, including a first ingate 4a, a second ingate 4b, a third ingate 4c, and a fourth ingate 4d. The connection between the runner 3 and the four ingates is designed with a rounded corner of radius R1 = 30mm. The flow direction in the runner 3 is at the same angle (120°) to the flow direction in the four ingates. The vertical runner section from the end of the ingates to the guide vane forming cavity is called the ingate 6, including the first ingate 6a, the second ingate 6b, the third ingate 6c, and the fourth ingate 4d. The ingate is 6d; the casting consists of two identical double-bladed guide vanes (i.e., the blade body contains two blades). The guide vanes are made of K417 nickel-based superalloy (i.e., nickel-based precipitation-hardening equiaxed crystal casting superalloy). Taking one guide vane as an example, the guide vane includes an upper edge plate 7, a blade body 8, and a lower edge plate 9. The lower edge plate 9 includes two parallel thick-walled sections (i.e., the first rib S1 and the second rib S2). The end section of the first ingate 4a (i.e., the first ingate 6a) is connected to the first rib S1. The end section of the second ingate 4b (i.e., the second ingate 6b) is connected to the second stiffener S2, thus forming a stepped ingate. The cross-sectional thickness of the first ingate 6a and the second ingate 6b is 60% of the thickness of the first or second stiffener of the guide vane. The longitudinal section of the ingate 6 is a trapezoid with a base length of 60-75mm, a height of 35mm on one side and 55mm on the other side. Furthermore, the connection between the four ingates and the horizontal section of the ingate is designed with a rounded transition with a radius of R2 = 8mm.

[0074] The gating system uses thermal insulation cotton for molding. The material of the thermal insulation cotton is aluminum silicate, and the thickness of each layer of thermal insulation cotton is 20mm. Among them, the main gating 2 uses one layer of thermal insulation cotton, and the gating cup 1, the horizontal gating 3 and the inner gating 4 all use two layers of thermal insulation cotton. The forming cavity of the guide blade 5 is defined as the first part and the second part along the flow direction of the molten metal (from the bottom to the top). The length ratio of the first part to the second part in the vertical direction is 1:1. First, a layer of thermal insulation cotton is designed as a whole from the top to the bottom of the forming cavity of the guide blade 5. Then, half a layer of thermal insulation cotton is added from 1 / 2 to the bottom of the forming cavity of the guide blade 5. That is, a half layer of thermal insulation cotton is set from 1 / 2 to the bottom of the forming cavity of the guide blade 5.

[0075] When applying the above-mentioned high-temperature alloy guide vane casting system, vacuum melting casting is preferred, but not limited to, the following process parameters:

[0076]

[0077] Example 2

[0078] The gating system for the high-temperature alloy guide vane in this embodiment is the same as that in Embodiment 1, except that the connection between the horizontal gating 3 and the four ingates is designed with a rounded corner with a radius of R1 = 50 mm.

[0079] Example 3

[0080] The gating system for the high-temperature alloy guide vane in this embodiment is the same as that in Embodiment 1, except that the connection between the horizontal gating 3 and the four ingates is designed with a rounded corner with a radius of R1 = 80 mm.

[0081] Comparative Example 1

[0082] The casting system of the high-temperature alloy guide vane in this comparative example is the same as that in Example 1. The difference is that the fillet R1 at the connection between the horizontal runner and the four ingates in this comparative example is 5mm. After actual casting, the guide vane has visible shrinkage defects (greater than 10mm). The porous interior and surface of the guide vane cannot meet the quality requirement that defects of less than 1.0mm are allowed.

[0083] Comparative Example 2

[0084] The casting system for the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that the main gating system does not employ the insulation method described in this invention. After actual casting, the guide vane exhibits visible shrinkage cavities (greater than 10 mm), and the guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are permitted.

[0085] Comparative Example 3

[0086] The casting system of the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that: the pouring cup 1, the horizontal runner 3 and the inner runner 4 are all made of two layers of insulation cotton, while the main runner 2 is made of only 0.5 layers of insulation cotton. After actual casting, the guide vane has visible shrinkage defects (greater than 10 mm). The guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are allowed.

[0087] Comparative Example 4

[0088] The casting system of the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that: the pouring cup 1, the horizontal runner 3 and the inner runner 4 are all made of two layers of insulation cotton, and the main runner 2 is made of 2.5 layers of insulation cotton. After actual casting, the guide vane has visible shrinkage defects (greater than 10 mm). The guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are allowed.

[0089] Comparative Example 5

[0090] The casting system for the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that the heat preservation method in the forming cavity of guide vane 5 is not used. After actual casting, the guide vane has visible shrinkage defects (greater than 10 mm), and the guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are allowed.

[0091] Comparative Example 6

[0092] The casting system for the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that the molding cavity of the guide vane 5 is designed with only one layer of insulation cotton. After actual casting, the guide vane has visible shrinkage defects (greater than 10 mm), and the guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are allowed.

[0093] Comparative Example 7

[0094] The casting system for the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that the molded cavity of guide vane 5 is only designed with a half-layer of insulation cotton from 1 / 2 to the bottom, and the remaining parts of the molded cavity of guide vane 5 are not insulated. After actual casting, the guide vane has visible shrinkage defects (greater than 10mm), and the guide vane does not meet the quality requirement that internal and surface defects of less than 1.0mm are allowed.

[0095] Comparative Example 8

[0096] The gating system of the high-temperature alloy guide vane in this comparative example is the same as that in Example 1, except that the ingate does not adopt a stepped design, and the ingate is only opened at the first or second stiffener. After actual casting, the guide vane has visible shrinkage defects (greater than 10 mm), and the guide vane does not meet the quality requirement that internal and surface defects of less than 1.0 mm are allowed.

[0097] The guide vanes prepared in Examples 1-3 are as follows: Figure 8 As shown, the guide vanes prepared in Comparative Examples 1-8 are as follows: Figure 9 As shown, it is clear that, compared with comparative examples 1-8, the embodiments provided by the present invention can effectively avoid defects such as insufficient casting, shrinkage cavities, shrinkage porosity, and cracks, thereby improving the yield and dimensional accuracy.

[0098] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A casting system for high-temperature alloy guide vanes, characterized in that, The gating system includes a gating system and guide vane forming cavities. The guide vane forming cavities are symmetrically arranged on both sides of the gating system, forming a two-piece structure, and is used in a bottom-pouring method. The gating system consists of a pouring cup, a main gating system, a runner, and ingates. The pouring cup is connected to the main gating system and is distributed vertically. The lower end of the main gating system is connected to the middle of the runner. M ingates are symmetrically arranged on the left and right sides of the runner. The angle between the liquid flow direction in the runner and the liquid flow direction in the M ingates is the same and is 120°. The bottoms of the runner and the M ingates are flush. Each connection point between the ingate and the runner is designed with a fillet of radius R1, satisfying 30mm≤R1≤80mm; The vertical runner between the end of the ingate and the forming cavity of the guide vane is called the ingate. The guide vane includes an upper edge plate, a blade body, and a lower edge plate. The lower edge plate includes N parallel thick-walled sections, each of which is provided with an ingate. The cross-sectional thickness of the ingate is 50-80% of the thickness of the thick-walled section of the guide vane. The number of thick-walled portions of the guide vanes and the number of ingates satisfy the following condition: M=N≥4; Where M is the number of ingates; N represents the number of thick-walled sections of the guide vane; The connection between the ingate and the horizontal section of the ingate is designed with a rounded transition of radius R2. The rounded corner R2 helps to reduce flow resistance and allows the molten metal to fill the cavity as quickly as possible. The value of R2 is 5 to 10 mm. The ingate opened on the same guide vane forming cavity adopts a stepped design and is connected and matched with the thick-walled part of the guide vane to form a stepped ingate. This ensures that the ingate provides sufficient feeding for each thick-walled part in the guide vane, reduces the defects of loose shrinkage cavities in the guide vane, and improves the quality of the guide vane. The main gating system uses W layers of insulation cotton, and the pouring cup, runner, and ingate use Z layers of insulation cotton, satisfying: Z=a W, where a represents the proportionality coefficient, and a takes at least one value from 1, 1.5 or 2, and W is a natural number greater than or equal to 1; The guide vane forming cavity is defined as a first part and a second part along the direction of molten metal flow. The first part is closer to the ingate, and the second part is farther from the ingate. The first part uses X layers of insulation cotton, and the second part uses Y layers of insulation cotton, satisfying X=1.

5. Y, where Y is a natural number greater than or equal to 1; the length ratio of the first part to the second part of the guide vane forming cavity in the vertical direction is 1:

1.

2. The casting system for high-temperature alloy guide vanes according to claim 1, characterized in that, The main gating system uses W layers of insulation cotton, and the pouring cup, runner, and ingate use Z layers of insulation cotton, satisfying: Z=a W, where a represents the proportionality coefficient, and a takes at least one value of 1, 1.5 or 2, and W=1.

3. The casting system for high-temperature alloy guide vanes according to claim 1, characterized in that, The guide vane forming cavity is defined as a first part and a second part along the direction of molten metal flow. The first part uses X layers of insulation cotton, and the second part uses Y layers of insulation cotton, satisfying X=1.

5. Y, where Y=1.

4. The casting system for high-temperature alloy guide vanes according to any one of claims 1-3, characterized in that, The number of thick-walled portions of the guide vanes and the number of ingates satisfy the following condition: M=N=4; Where M is the number of ingates; N represents the number of thick-walled sections of the guide vane.

5. The casting system for high-temperature alloy guide vanes according to claim 1, characterized in that, The insulation material includes at least one of asbestos, aluminum silicate, and calcium silicate.

6. The casting system for high-temperature alloy guide vanes according to claim 1, characterized in that, The guide vane is made of at least one of nickel-based, titanium-based, and cobalt-based high-temperature alloys.

7. The application of a casting system for high-temperature alloy guide vanes according to any one of claims 1-6, characterized in that, It is applicable to the casting process of complex thin-walled high-temperature alloys with parallel thick-walled sections.

8. The application of the casting system for high-temperature alloy guide vanes according to claim 7, characterized in that, Applicable to the production process of guide vanes.

9. The application of the casting system for high-temperature alloy guide vanes according to claim 8, characterized in that, The guide vanes were prepared using a vacuum melting and casting method.

Citation Information

Patent Citations

  • Casting system design method for preventing root crack defect of inner gate of casting

    CN105598374A

  • Wax mould combination of turbine guide vane and precision casting method of wax mould combination

    CN107598097A

  • Gating system of guider blade blank

    CN115055645A