A copper tube micro-gap lap joint upward flooding brazing method
By using the micro-gap lap joint upward flow brazing method for copper tubes, and by heating at high points and filling with brazing filler metal at low points, the operational difficulty and weld leakage problem of all-position brazing of copper tubes are solved, achieving high-quality, labor-saving, material-saving and environmentally friendly welding results.
Patent Information
- Application Number
- CN202311577074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-23
AI Technical Summary
In industrial installation projects, all-position brazing of copper pipes is difficult, and weld leakage is a common problem. Poor weld formation leads to quality issues such as insufficient weld length, lack of fusion, weld beads, and leakage.
The copper tube micro-gap lap joint upward flow brazing method is adopted. By heating at high points and filling with brazing filler metal at low points, the liquid brazing filler metal is rapidly wetted and filled upward in the micro-gap area through the smoke window effect and capillary action, forming a weld of uniform height.
It reduces the operational difficulty of all-position brazing, eliminates common quality defects such as weld leakage, improves weld quality, and achieves the effects of saving labor and materials as well as energy conservation and environmental protection.
Smart Images

Figure CN117733264B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of industrial installation engineering technology, and in particular to a brazing method for upward flow brazing of copper tube micro-gap lap joints. Background Technology
[0002] In practical industrial installation engineering, all-position brazing of fixed socket joints is quite difficult. In some cases, the welder's operating skills are inadequate, and they often only braze the fillet weld of the copper pipe joint without fully filling the lap gap. In other cases, the welder does not have a good grasp of the all-position flame brazing technique for socket joints, resulting in insufficient filler metal length or poor fusion of the lap weld. This can easily lead to difficulty in controlling the filling of the gap and the weld formation at the lap joint. Both of these situations can easily cause quality problems such as insufficient brazing length of the lap weld, lack of fusion, weld beads, and leakage. Summary of the Invention
[0003] The purpose of this application is to at least solve one of the technical problems existing in the prior art. To this end, this application proposes a copper tube micro-gap lap joint upward flow brazing method, which can reduce the operational difficulty of all-position brazing, eliminate the common quality defect of weld leakage as much as possible, and achieve the goals of ensuring weld aesthetics, improving quality, saving labor and materials, and saving energy and environmental protection.
[0004] The copper tube micro-gap lap joint upward flow brazing method according to the first aspect of this application includes the following steps:
[0005] The insertion port of the insert tube is inserted into the socket of the socket tube along the first direction to complete the socket connection. A gap area is formed between the socket and the insert tube. The two ends of the gap area along the first direction are sequentially defined as a lower overlap interface and an upper overlap interface.
[0006] Fix the socket and the insertion tube relative to each other;
[0007] The insert and the socket are alternately and uniformly heated with a welding torch until a relative temperature difference is formed, wherein the temperature of the socket is higher than that of the insert, and the insert is heated to a temperature suitable for melting the brazing filler metal.
[0008] The lower interface is filled with brazing filler metal as an inlet, and after the brazing filler metal is melted, it flows upward along the higher temperature point in the gap area until it fills the gap area and overflows the upper interface.
[0009] Backfill the weld leg to a position lower than the lower lap joint, and weld it into a lap fillet weld of uniform height;
[0010] Remove the welding torch to allow the liquid brazing filler metal to solidify, thus completing the brazing process.
[0011] The copper tube micro-gap lap joint upward flow brazing method according to the first aspect of this application has at least the following beneficial effects: Upward flow flame brazing is performed by heating at high points and filling with brazing filler metal at low points. Under the combined action of the smoke window effect and the capillary action in the micro-gap region, the molten liquid brazing filler metal quickly wets and fills the welded lap surface. Simultaneously, the uniform height of the weld leg ensures complete filling, enabling rapid completion of the upward flow brazing process. This method can complete the filling of the lap gap in a single operation, reducing the operational difficulty of all-position brazing, minimizing common weld leakage defects, and achieving the goals of improving quality, saving labor and materials, and saving energy and protecting the environment.
[0012] According to the copper tube micro-gap lap joint upward diffused brazing method described in the first aspect of this application, the method of alternating and uniformly heating the insert and the socket tube by a welding torch includes: using the outer flame at the end of the flame core for heating during brazing, first heating the insert tube and then heating the socket tube, and continuously moving the flame up and down while simultaneously making a circular motion during heating.
[0013] According to the copper tube micro-gap lap joint upward flow brazing method described in the first aspect of this application, with the position of the socket connection as the reference, let L be the range of vertical movement when heating the insert tube and the socket tube respectively, and let L satisfy the following relationship: 20mm≤L≤50mm.
[0014] According to the copper tube micro-gap lap joint upward flow brazing method described in the first aspect of this application, the insert tube is adapted to be heated to between 740°C and 760°C, and the receiving tube is adapted to be heated to between 780°C and 810°C.
[0015] According to the copper tube micro-gap lap joint upward diffused brazing method described in the first aspect of this application, the filler metal feeding position is offset from the flame of the welding torch along the circumference of the inserted tube by a certain angle.
[0016] According to the copper tube micro-gap lap joint upward flow brazing method described in the first aspect of this application, the first direction is a vertical direction, the support tube and the insert tube are fixed relative to each other and vertically arranged, and the insert tube is located below the support tube, and brazing filler metal is filled along the circumference of the lower lap joint.
[0017] According to the copper tube micro-gap lap joint upward diffused brazing method described in the first aspect embodiment of this application, three trisection points are found at the lower lap joint with the center of the socket as a reference, and the brazing filler metal is uniformly filled at the positions of 1 to 3 trisection points as immersion points.
[0018] According to the copper tube micro-gap lap joint upward flow brazing method of the first aspect embodiment of this application, the first direction is the horizontal direction, the support tube and the insertion tube are fixed relative to each other and set horizontally, the brazing filler metal is filled along the curved surface of the tube wall of the insertion tube and the fillet weld is fully filled, wherein the range of the brazing filler metal is an arc path with a preset arc centered at the lowest end of the lower lap joint.
[0019] According to the copper tube micro-gap lap joint upward flow brazing method described in the first aspect of this application, the range of the filler metal is an arc of 1 / 3 circumference or an arc of 1 / 4 circumference.
[0020] According to the copper tube micro-gap lap joint upward flow brazing method described in the first aspect embodiment of this application, the size of the gap area between the socket tube and the insert tube is 0.1mm to 0.2mm.
[0021] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0022] The present application will be further described below with reference to the accompanying drawings and embodiments;
[0023] Figure 1 This is a schematic diagram of a vertically arranged socket according to an embodiment of this application;
[0024] Figure 2 This is a schematic diagram illustrating the flow of solder when the socket is vertically positioned according to an embodiment of this application.
[0025] Figure 3 This is a schematic diagram of the structure of the socket and the insert after they are fixed relatively and vertically arranged according to an embodiment of this application;
[0026] Figure 4 for Figure 3 A cross-sectional view perpendicular to the axial direction at the socket connection position;
[0027] Figure 5 This is a schematic diagram of the vertically arranged socket and insert after brazing, according to an embodiment of this application.
[0028] Figure 6 A schematic diagram illustrating the horizontal configuration of the socket in an embodiment of this application;
[0029] Figure 7 A schematic diagram illustrating the flow of solder when the socket is horizontally positioned according to an embodiment of this application.
[0030] Figure 8 This is a schematic diagram of the structure of the socket and insert after they are fixed in a horizontal position according to an embodiment of this application.
[0031] Figure label:
[0032] 100. Pipe; 110. Socket;
[0033] 200. Intubation; 210. Intubation port;
[0034] 300, Gap area; 310, Lower interface; 320, Upper interface;
[0035] 400. Brazing filler metal; 410. Solder lead;
[0036] 500. Welding torch. Detailed Implementation
[0037] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.
[0038] In the description of this application, it should be understood that the orientation descriptions, such as up, down, front, back, left, right, etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0039] In the description of this application, "several" means one or more, "more than" means at least two, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is for the purpose of distinguishing technical features only and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.
[0040] In the description of this application, unless otherwise expressly defined, terms such as "setup," "installation," and "connection" should be interpreted broadly. Those skilled in the art can reasonably determine the specific meaning of the above terms in this application after considering the specific content of the technical solution.
[0041] Reference Figures 1 to 8 The copper tube micro-gap lap joint upward flow brazing method of the first aspect of this application is applied to solve the comprehensive technical problems of insufficient filler metal 400 filling length or poor fusion of the lap weld when welding socket copper tubes in high-difficulty all-position brazing, as well as obtaining an aesthetically pleasing weld appearance. This eliminates common weld leakage quality defects and ensures the manufacturing and installation quality of hot water systems, air conditioning refrigeration systems, cold storage refrigeration systems, and industrial equipment systems. The copper tube micro-gap lap joint upward flow brazing method includes the following steps:
[0042] The insertion port 210 of the insertion tube 200 is inserted into the socket port 110 of the socket tube 100 along the first direction to complete the socket connection. A gap region 300 is formed between the socket port 110 and the insertion tube 200. The two ends of the gap region 300 along the first direction are defined as the lower interface 310 and the upper interface 320 respectively.
[0043] Fix the socket 100 and the insertion tube 200 relative to each other;
[0044] The insertion tube 200 and the socket tube 100 are alternately and uniformly heated by the welding torch 500 until a relative temperature difference is formed, wherein the temperature of the socket tube 100 is higher than the temperature of the insertion tube 200, and the insertion tube 200 is heated to a temperature suitable for melting the brazing filler metal 400.
[0045] The lower point region along the direction of gravity in the lower interface 310 is used as the inlet to fill the brazing filler metal 400. After the brazing filler metal 400 is melted, it flows upward along the higher temperature point in the gap region 300 until it fills the gap region 300 and overflows the upper interface 320.
[0046] Backfill the weld leg 410 to a position where the height is lower than the lower lap joint 310, and weld it into a lap fillet weld of uniform height;
[0047] Remove the welding torch 500 to allow the liquid brazing filler metal 400 to solidify, thus completing the brazing process.
[0048] It should be noted that the brazing method of this application achieves the filling of the lapped micro-gap by overlapping copper tubes, heating at a high point of the flame, and filling the lapped micro-gap with brazing filler metal 400 at a low point. During brazing, when the temperature at the lower lapped joint 310 reaches the point where the brazing filler metal 400 can be melted, the flame of the welding torch 500 is moved to the socket 110 above the upper lapped joint 320 to continue heating. Then, brazing filler metal 400 is filled into the lower lapped joint 310, which is at a lower temperature than the heating point. During brazing, the molten liquid brazing filler metal 400 rapidly flows upward along the high-temperature point in the cavity of the lapped micro-gap until it completely fills the lapped gap and overflows from the upper lapped joint 320 inside.
[0049] Understandably, the insertion tube 200 should be heated to a temperature at least sufficient to melt the brazing filler metal 400. The brazing filler metal 400 is preferably a low-melting-point copper-based brazing filler metal 400. The relative temperature difference should be sufficient to create a chimney effect (thermal pressure), so that a high-temperature point is formed at the upper position. Combined with the capillary action of the pre-set gap area 300, the liquid brazing filler metal 400 can quickly wet and fill the welded joint surface along the heated high-temperature point. This method is simple to operate and can effectively prevent leakage at the welded joint due to insufficient filling or poor fusion of the brazing filler metal 400.
[0050] Reference Figures 1 to 8The copper tube micro-gap lap joint upward flow brazing method of the first aspect of this application adopts the method of heating at high point and filling the brazing filler metal 400 at low point to perform upward flow flame brazing. Under the dual action of the smoke window effect and the capillary action of the micro-gap region 300, the molten liquid brazing filler metal 400 quickly wets and fills the lap joint surface to be welded. At the same time, the uniform height of the weld foot 410 ensures that the interior is indeed filled, realizing the rapid completion of the upward flow brazing process. This method can complete the filling of the lap gap in one operation step, reducing the operation difficulty of all-position brazing, eliminating the common quality defects of weld leakage as much as possible, and achieving the purpose of improving quality, saving labor and materials, and saving energy and environmental protection.
[0051] It should be noted that the main steps for completing the welding of the socket joint include:
[0052] Step 1: Preheat the socket joint to the set brazing temperature;
[0053] Step 2: Heat the high point and fill the low point with brazing filler metal 400 mm to complete the filling of the lap gap;
[0054] Step 3: Backfill the slightly lower outer lap joint area of the weld leg 410 and weld it into a lap fillet weld with a uniform weld leg height of 410.
[0055] In some embodiments of this application, the method of alternating and uniformly heating the insertion tube 200 and the receiving tube 100 by the welding torch 500 includes: using the outer flame at the end of the flame core for heating during brazing, heating the insertion tube 200 first and then heating the receiving tube 100, and continuously moving the flame up and down while making a circular motion during heating.
[0056] Understandably, specific references Figure 3 and Figure 8 The insert 200 and the socket 100 can be aligned and fixedly installed using temporary clips. During brazing, the outer flame at the end of the flame core is used to alternately and evenly heat the lower and upper tubes at the socket connection position. The heating torch angle is approximately horizontal. During heating, the lower tube is heated first, followed by the upper tube. The flame should be moved up and down and made in a circular motion to ensure that the insert 200 and the socket 100 are heated evenly.
[0057] In some embodiments of this application, specific references are made. Figure 3 and Figure 8 Based on the position of the socket connection, let L be the range of vertical movement when heating the insert 200 and the socket 100 respectively, where L satisfies the following relationship: 20mm≤L≤50mm. In some embodiments of this application, the insert 200 is suitable to be heated to between 740°C and 760°C, and the socket 100 is suitable to be heated to between 780°C and 810°C.
[0058] Understandably, the heating range should be approximately 20-50mm on both sides of the socket. Throughout the welding process, the overall temperature of the lower tube of the socket joint should be maintained at approximately 740-760℃, and the overall temperature of the upper tube at approximately 780-810℃, with a temperature difference of approximately 20-40℃ between the upper and lower tubes. This satisfies both the requirement to melt the brazing filler metal to 400℃ and the requirement to create a fume window effect.
[0059] In some embodiments, specific references are made. Figure 2 and Figure 7 Before filling the brazing filler metal 400, in addition to observing and controlling the temperature of the upper and lower tubes, the flame heating position when filling the brazing filler metal 400 must be outside the socket 110 of the upper tube, as shown in the figure, in order to achieve the best filling effect.
[0060] In some embodiments of this application, specific references are made. Figure 4 The filler metal 400 is positioned at a certain angle relative to the flame heated by the welding torch 500 along the circumference of the insertion tube 200. It is understood that when filling the filler metal 400, it is preferable to fill it from the other side, avoiding direct contact between the welding torch flame and the flat filler metal 400, which could cause premature melting and phosphorus burn-off.
[0061] In some embodiments, the circumference of the cannula 100 or the insertion tube 200 can be evenly divided into multiple regions, as detailed in the following examples. Figure 4 It forms 6 zones, which are defined as zones 1-6 in clockwise order. When the welding torch is heating in zones 1 / 3 / 5, the filler metal 400 can be filled in zones 2 / 4 / 6, or in zones 4 / 6 / 2, depending on the adaptability of the actual construction environment.
[0062] In some embodiments of this application, specific references are made. Figures 1 to 5 The first direction is vertical. After the socket 100 and the insert 200 are fixed relative to each other, they are set vertically, and the insert 200 is located below the socket 100. The brazing filler metal 400 is filled along the circumference of the lower interface 310. Preferably, three trisection points are found at the lower interface 310 with the center of the insert 210 as the reference, and the brazing filler metal 400 is evenly filled at the positions of 1 to 3 trisection points as the feeding points.
[0063] Understandably, the tip of the brazing filler metal 400 flat strip is aligned with and lightly pressed onto the gap area 300, where it is melted by the heat from the upper pipe edge. The filler metal 400 is then fed along the circumference of the pipe using 1-3 feeding points. The welding torch 500 continues to heat the pipe circumference, maintaining a temperature of 780-810°C, and moving the highest heating point along the circumference to a higher position. This allows the liquid brazing filler metal 400 to rapidly wet the welded lap surface in both horizontal and upward directions along the micro-gap area 300, filling it completely until the liquid brazing filler metal 400 fills the entire lap gap and overflows into the upper lap joint 320. This process of filling the entire lap gap of the joint is completed in one operation, quickly completing the upward flow brazing process. Once the liquid brazing filler metal 400 fills the pipe to the upper lap joint 320 and forms a suitable lap weld leg 410 height, the filler metal 400 is withdrawn.
[0064] After completing the filling step of the overlap gap, refer to the following for details. Figure 5 If the height of the weld leg 410 in the weld area is found to be insufficient, after the joint temperature drops slightly, the outer lap joint area where the height of the weld leg 410 is slightly lower should be backfilled appropriately to form a lap fillet weld of uniform height. When the welding torch 500 is removed from the welded joint, the liquid brazing filler metal 400 inside and outside the gap will solidify rapidly, thereby generating a full-welded, high-quality permanent lap weld.
[0065] In some embodiments of this application, specific references are made. Figures 6 to 8 The first direction is horizontal. After the socket 100 and the insert 200 are fixed relative to each other, they are set horizontally. The filler metal 400 is filled along the curved surface of the insert 200 wall to fully fill the fillet weld. The range of the filler metal 400 is an arc path with a preset arc radius centered on the lowest end of the lower joint 310. Preferably, the range of the filler metal 400 is an arc of 1 / 3 or 1 / 4 of the circumference.
[0066] It is understandable that during brazing, the flow direction of the liquid filler metal 400 is primarily due to the combined force of the horizontal and upward directions, which wet and fill the metal. See the specific reference... Figure 7 It wets both horizontally and upwards, and through high-point heating and low-point filling of the brazing filler metal, it is ultimately transformed into upward diffused welding.
[0067] In some embodiments, the horizontal socket joint is brazed and fixed in a similar manner to the vertical arrangement described above. The difference is that when the temperature of the insert 200 reaches approximately 740–760°C and the temperature of the socket 100 reaches 780–810°C, the flame is moved to the highest point of the top region of the horizontal socket joint for heating. Then, filler metal 400 is fed into the bottom region of the socket joint (approximately 5–7 o'clock). When filler metal 400 overflows and forms a small fillet weld at the lap joint 320 on the top of the pipe, the filling process of the lap gap is complete. The welding torch 500 is moved back and forth on the top of the socket 100 and the insert 200 to replenish the temperature and maintain the original brazing temperature. At this time, attention is focused on the bottom section of the pipe. The fillet weld is filled in full along the clock position from 5 o'clock to 8 o'clock in the bottom of the pipe by drawing an arc. If the fillet weld leg 410 of other parts of the joint circumference is insufficient, it is appropriately returned to the uniform weld leg 410 height to complete the brazing of the entire fixed horizontal socket joint.
[0068] In some embodiments of this application, the size of the gap region 300 between the socket 100 and the insert 200 is 0.1 mm to 0.2 mm. It is understood that the size of the gap region 300 needs to be limited in order to satisfy the brazed joint form of a micro-gap lap joint and to utilize capillary action for better formation. In other embodiments, the size of the gap region can also be adaptively adjusted as the diameters of the socket 100 and the insert 200 change.
[0069] In some embodiments of this application, specific references are made. Figures 1 to 8 A method for upward diffused brazing of copper tube micro-gap lap joints includes connecting copper tubes with an overhead socket and a horizontal socket in a fixed socket joint in all positions. After temporary clamps are aligned and fixed, a low-melting-point copper-based brazing filler metal 400 and a socket micro-gap lap joint are selected. The key welding technology of high-point heating and low-point filling of brazing filler metal 400 is used for upward diffused flame brazing. Because the insert 200 of the socket joint is heated to 740-760°C and the socket 100 is heated to 780-810°C, a relative temperature difference is formed between the two welded parts. The socket 100 is hotter than the insert 200. Taking advantage of the special temperature and temperature difference at this time, the brazing filler metal 400 is fed into the lap joint (the fixed overhead socket is filled with brazing filler metal 400 in the circumference of its lap joint; the fixed horizontal socket is filled with brazing filler metal 400 in the lap joint area at the bottom of its pipe). Under the dual action of the smoke window effect (thermal pressure) and the capillary action of the micro-gap, the molten liquid brazing filler metal 400 is simultaneously moved horizontally and upward. In the cavity of the lap joint micro-gap, it quickly flows upward along the high temperature point to fill and wet the welded lap joint surface until it completely fills the micro-gap and overflows from the inner lap joint.
[0070] After completing the filling step of the lap gap, backfill the part where the height of the outer lap joint weld foot 410 is slightly lower, and weld the lap fillet weld with a uniform height. When the welding gun 500 is removed from the welded joint, the liquid brazing filler metal 400 inside and outside the gap quickly solidifies, thereby generating a full-welded high-quality lap weld.
[0071] It is understood that this application provides embodiments of vertical and horizontal arrangement of the socket 100 and insert 200 after they are relatively fixed. In other embodiments, the socket 100 and insert 200 can be tilted after they are relatively fixed, wherein the filling method of the brazing filler metal 400 can refer to the method when the socket 100 and insert 200 are relatively fixed and horizontally arranged. Only the arc path of the filling brazing filler metal 400 needs to be adjusted specifically. Similarly, relying on the smoke window effect and capillary action, the liquid brazing filler metal 400 can quickly wet and fill the welded lap surface along the high-temperature heating point.
[0072] The technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0073] The embodiments of this application have been described in detail above with reference to the accompanying drawings. However, this application is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of this application.
Claims
1. A method for upward flow brazing of micro-gap joints in copper tubes, characterized in that, Includes the following steps: The insertion port of the insert tube is inserted into the socket of the socket tube along the first direction to complete the socket connection. A gap area is formed between the socket and the insert tube. The two ends of the gap area along the first direction are sequentially defined as a lower overlap interface and an upper overlap interface. Fix the socket and the insertion tube relative to each other; The insert and the socket are alternately and uniformly heated with a welding torch until a relative temperature difference is formed, wherein the temperature of the socket is higher than that of the insert, and the insert is heated to a temperature suitable for melting the brazing filler metal. When the temperature of the lower interface reaches a temperature suitable for melting the brazing filler metal, the flame of the welding torch is moved to the socket position above the upper interface to continue heating; The lower interface, with a temperature lower than the heating point, is used as an inlet for filling with brazing filler metal along the direction of gravity. After the brazing filler metal is melted, it flows upward along the higher temperature point in the gap area until it fills the gap area and overflows from the upper interface. After the gap area is filled, the weld foot is backfilled to a height lower than the lower lap joint, and then welded into a lap fillet weld of uniform height. Remove the welding torch to allow the liquid brazing filler metal to solidify, thus completing the brazing process.
2. The copper tube micro-gap lap joint upward flow brazing method according to claim 1, characterized in that: The method of alternating and uniformly heating the insert and the socket with a welding torch includes: using the outer flame at the end of the flame core for heating during brazing, heating the insert first and then heating the socket, and continuously moving the flame up and down while making a circular motion during heating.
3. The copper tube micro-gap lap joint upward flow brazing method according to claim 2, characterized in that: Based on the position of the socket connection, let L be the range of vertical movement when heating the insert and the socket respectively. L satisfies the following relationship: 20mm ≤ L ≤ 50mm.
4. The copper tube micro-gap lap joint upward flow brazing method according to claim 2, characterized in that: The cannula is suitable for being heated to between 740°C and 760°C, and the receiving tube is suitable for being heated to between 780°C and 810°C.
5. The copper tube micro-gap lap joint upward flow brazing method according to claim 1, characterized in that: The position of the brazing filler metal is offset from the flame of the welding torch along the circumference of the insertion tube by a certain angle.
6. The copper tube micro-gap lap joint upward flow brazing method according to claim 5, characterized in that: The first direction is the vertical direction. The socket and the insert are fixed relative to each other and set vertically. The insert is located below the socket and the brazing filler metal is filled along the circumference of the lower interface.
7. The copper tube micro-gap lap joint upward flow brazing method according to claim 6, characterized in that: Using the center of the socket as a reference, find three trisection points at the lower interface, and use the positions of 1 to 3 trisection points as feeding points to evenly fill the brazing filler metal.
8. The copper tube micro-gap lap joint upward flow brazing method according to claim 5, characterized in that: The first direction is horizontal. After the support tube and the insertion tube are fixed relative to each other, they are set horizontally. The filler metal is filled along the curved surface of the tube wall and the fillet weld is fully filled. The range of the filler metal is an arc path with a preset arc value centered at the lowest end of the lower joint.
9. The copper tube micro-gap lap joint upward flow brazing method according to claim 8, characterized in that: The filler metal is applied to an arc of 1 / 3 or 1 / 4 of the circumference.
10. The copper tube micro-gap lap joint upward flow brazing method according to claim 1, characterized in that: The size of the gap between the socket and the insertion tube is 0.1 mm to 0.2 mm.
Citation Information
Patent Citations
Copper pipe socket brazed connection construction method
CN103600147A