A large composite high-chromium steel roll surfacing repair reformed layer and a preparation method thereof

By layer-by-layer welding of the bottom layer, transition layer and working layer on the high-chromium steel roll, combined with heat treatment, the problem of the difficulty in repairing high-chromium steel composite vertical rolls has been solved, realizing efficient and economical roll remanufacturing, reducing production costs and extending service life.

CN117733404BActive Publication Date: 2026-11-20YANSHAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311855353.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-20
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

High-chromium steel composite vertical rolls have high manufacturing costs, a high tendency to harden, strong crack sensitivity, and poor weldability, making it difficult to successfully repair by overlay welding. As a result, vertical rolls worn to the failure size need to be re-composite and remanufactured, increasing the procurement costs for steel mills.

Method used

The repair and reconstructed layer is made of large composite high-chromium steel rolls, including the base surface, the underlayer, the transition layer and the working layer. The repair layer is formed by welding layer by layer with flux-cored wire and heat treatment to meet the requirements of rolling.

Benefits of technology

It extends the service life of the rolls, reduces production costs, improves performance, and is simple to use. It is not limited by the size of the rolls, has a high cost-performance ratio, and is suitable for the repair and remanufacturing of large composite high-chromium steel rolls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application belongs to the technical field of metal surface treatment, and particularly relates to a large composite high-chromium steel roller surfacing repair remanufacturing layer and a preparation method thereof. The application provides a large composite high-chromium steel roller surfacing repair remanufacturing layer, which comprises a base surface, a primer layer, a transition layer and a working layer connected in sequence, the primer layer is formed by surfacing with a primer layer flux-cored wire, the transition layer is formed by surfacing with a transition layer flux-cored wire, and the working layer is formed by surfacing with a working layer flux-cored wire. The surfacing repair remanufacturing has high cost performance, not only prolongs the service life of the roller, but also greatly reduces the production cost of a steel plant (the surfacing repair composite high-chromium steel roller can reduce the cost by 30%-50%).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of metal surface treatment technology, and in particular relates to a large composite high-chromium steel roll overlay repair and remodeling layer and its preparation method. Background Technology

[0002] To improve the performance of vertical rolls in hot-rolled strip mills, some domestic steel mills have adopted high-chromium steel composite vertical rolls. These rolls offer superior throughput, wear resistance, strip edge quality, and production efficiency compared to alloy-cast and semi-steel vertical rolls. However, high-chromium steel composite vertical rolls are not only expensive to manufacture, but also have a high hardening tendency (carbon content 1.2–1.8%, chromium content 11%–17%, and other trace alloying elements; hardness range is generally HS70–80), making them highly susceptible to cracking and extremely difficult to weld. Successful weld repair is extremely challenging, and vertical rolls worn to the point of failure are often re-composite and remanufactured, significantly increasing procurement costs for steel mills. Summary of the Invention

[0003] 1. Technical problems to be solved High-chromium steel composite vertical rolls are not only expensive to manufacture, but also have a high hardening tendency (carbon content 1.2-1.8%, chromium content 11%-17% and other trace alloying elements, hardness range generally HS70-80), strong crack sensitivity, and extremely poor weldability, making successful weld overlay repair difficult. Vertical rolls worn to the failure size are often re-composite and remanufactured, which increases the procurement costs for steel mills by a lot. This application provides a weld overlay repair remanufacture layer for large composite high-chromium steel rolls and its preparation method.

[0004] 2. Technical Solution To achieve the above objectives, this application provides a large composite high-chromium steel roll surfacing repair and remanufacturing layer, comprising a substrate surface, a base layer, a transition layer, and a working layer connected sequentially. The base layer is formed by surfacing with a base layer flux-cored welding wire, the transition layer is formed by surfacing with a transition layer flux-cored welding wire, and the working layer is formed by surfacing with a working layer flux-cored welding wire. The base layer flux-cored welding wire comprises the following components by weight percentage: C 0.03–0.08, Si 0.3–0.5, P / s 0.02–0.03, Mn 0.8–1.0, Cr 16–25, Ni 8–12, with alloying elements Mo+V++Ti 0.8–1.5, and the balance being Fe. The transition layer flux-cored welding wire comprises the following components by weight percentage: C 0.15–0.25, Si 0.3–0.5, P / s 0.02–0.03, Mn 1.0–1.5, Cr The working layer flux-cored wire consists of the following components by weight percentage: C 0.25-0.35, Si 0.3-0.5, P / s 0.02-0.03, Mn 1.2-1.8, Cr 12-15, Mo 2.0-3.0, Ni+V+W 4.0-6.0, and the balance Fe.

[0005] Another embodiment provided in this application is as follows: the hardness HSD of the underlayer is 30-40, the hardness HSD of the transition layer is 55-65, and the hardness HSD of the working layer is 65-75.

[0006] Another implementation method provided in this application is as follows: the base layer consists of 2 layers, the transition layer consists of 2 layers, and the working layer consists of several layers.

[0007] This application also provides a method for preparing the repair and remanufacturing layer of the large composite high-chromium steel roll. The method includes preheating the roll, placing the preheated roll on a welding machine, welding the bottom layer flux-cored wire on the preheated roll in proportion to form a bottom layer, welding the transition layer flux-cored wire on the bottom layer in proportion to form a transition layer, welding the working layer flux-cored wire on the transition layer in proportion to form a working layer, performing intermediate heat treatment when the thickness of the weld layer on one side reaches 20-30 mm, performing final heat treatment after the welding is completed, and grinding the roll after the final heat treatment to complete the repair and remanufacturing of the roll.

[0008] Another embodiment provided in this application is as follows: the preheating temperature is 500℃, the heating rate is 20℃ / h, the heating time is 25 hours, the holding temperature is 500℃, the holding time is calculated according to the roller diameter mm / 60, and the temperature is kept uniform by using an axial flow fan for internal circulation.

[0009] Another embodiment provided in this application is as follows: the intermediate heat treatment temperature is 520℃, the heating rate is 20℃ / h, the holding time is calculated according to the roller diameter mm / 60, the cooling rate is not greater than 20℃ / h, the internal circulation of the axial flow fan is used to maintain uniform temperature, and when the temperature drops to 400℃, the secondary overlay welding is performed.

[0010] Another embodiment provided in this application is as follows: the final heat treatment temperature is 520℃, the heating rate is 20℃ / h, the holding time is calculated according to the roller diameter mm / 60, the cooling rate is not greater than 20℃ / h, the internal circulation of the axial flow fan is used to maintain uniform temperature, and the furnace door is opened when the temperature drops to less than 80℃.

[0011] Another embodiment provided in this application is as follows: the interlayer temperature of each working layer is 260-350°C, the interlayer temperature of each base layer is 260-350°C, and the interlayer temperature between adjacent working layers and the base layer is 260-350°C.

[0012] Another embodiment provided in this application is that the thickness of the working layer or the base layer is 4.5 to 6.5 mm.

[0013] 3. Beneficial effects Compared with existing technologies, the beneficial effects of the large composite high-chromium steel roll weld overlay repair and remodeling layer and its preparation method provided in this application are as follows: The large composite high-chromium steel roll welding repair and remanufacturing layer provided in this application realizes the welding repair and remanufacturing of high-chromium steel vertical rolls, filling the gap in domestic composite high-chromium steel roll welding repair.

[0014] The method for preparing the remanufactured layer of large composite high-chromium steel rolls provided in this application has a high cost-performance ratio for weld overlay repair and remanufacturing. It not only extends the service life of the rolls, but also greatly reduces the production cost of steel plants (the cost of composite high-chromium steel rolls repaired by weld overlay can be reduced by 30% to 50%).

[0015] The method for preparing the overlay repair and remanufacturing layer of large composite high-chromium steel rolls provided in this application involves simple equipment and processes, is easy to operate, and is not limited by roll size or construction site. It is suitable for the repair and remanufacturing of large composite high-chromium steel rolls, and its service life is close to or even reaches that of new rolls. The repaired and remanufactured large composite high-chromium steel rolls, after flaw detection, are free of welding defects such as slag inclusions, incomplete fusion, incomplete penetration, and cracks, and have a hardness of HSD65-70, fully meeting the requirements for roll rolling use. At the same time, this invention has a high cost-performance ratio, excellent matrix bonding strength, high-temperature wear resistance, and corrosion resistance, which can improve the performance of rolls and effectively extend their service life, showing broad application prospects and economic benefits. Detailed Implementation

[0016] The specific embodiments of this application will be described in detail below. Based on these detailed descriptions, those skilled in the art will be able to clearly understand and implement this application. Without departing from the principles of this application, features in various embodiments can be combined to obtain new implementations, or certain features in some embodiments can be substituted to obtain other preferred implementations.

[0017] This application provides a large composite high-chromium steel roll surfacing repair and remanufacturing layer, comprising a substrate surface, a base layer, a transition layer, and a working layer connected in sequence. The base layer is formed by surfacing with a base layer flux-cored welding wire, the transition layer is formed by surfacing with a transition layer flux-cored welding wire, and the working layer is formed by surfacing with a working layer flux-cored welding wire. The base layer flux-cored welding wire has the following weight percentage composition: C 0.03~0.08, Si 0.3~0.5, P / s 0.02~0.03, Mn 0.8~1.0, Cr 16~25, Ni 8~12, alloying elements Mo+V++Ti 0.8~1.5, and the balance being Fe. The transition layer flux-cored welding wire has the following weight percentage composition: C 0.15~0.25, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.0~1.5, Cr The working layer flux-cored wire consists of the following components by weight percentage: C 0.25-0.35, Si 0.3-0.5, P / s 0.02-0.03, Mn 1.2-1.8, Cr 12-15, Mo 2.0-3.0, Ni+V+W 4.0-6.0, and the balance Fe.

[0018] The present application discloses a large composite high-chromium steel roll overlay repair and remanufacturing technology method, which designs a three-layer overlay repair process. The overlay repair and remanufacturing layer is prepared by layering the prepared underlay, transition layer and working layer flux-cored welding wire onto the surface of the roll substrate. The underlay, transition layer and working layer are overlaid sequentially from the surface of the substrate outward.

[0019] Furthermore, the hardness HSD of the underlayer is 30-40, the hardness HSD of the transition layer is 55-65, and the hardness HSD of the working layer is 65-75.

[0020] Furthermore, the bottom layer consists of 2 layers, the transition layer consists of 2 layers, and the working layer consists of several layers.

[0021] This application also provides a method for preparing the repair and remanufacturing layer of the large composite high-chromium steel roll. The method includes preheating the roll, placing the preheated roll on a welding machine, welding the bottom layer flux-cored wire on the preheated roll in proportion to form a bottom layer, welding the transition layer flux-cored wire on the bottom layer in proportion to form a transition layer, welding the working layer flux-cored wire on the transition layer in proportion to form a working layer, performing intermediate heat treatment when the thickness of the weld layer on one side reaches 20-30 mm, performing final heat treatment after the welding is completed, and grinding the roll after the final heat treatment to complete the repair and remanufacturing of the roll.

[0022] Specifically, a method for preparing a reconstructed layer for welding repair of large composite high-chromium steel rolls includes the following steps: Step 1: Roll Preparation (1) Turning of the fatigue layer of the roll: the roll is turned by a minimum of 5mm on one side of the lathe, and the defective parts are cleaned up.

[0023] (2) The chemical composition of the shavings from the turning part is tested for C, S, P, Mn, Cr, Ni, Mo, V, W and Ti.

[0024] (3) Ultrasonic testing is used to inspect the roller surface for defects.

[0025] Step 2: Preparation of flux-cored welding wire (1) Preparation of the flux-cored wire for the underlayer: The composition of the flux-cored wire for the underlayer is prepared according to the alloy composition of the roll. The flux-cored wire for the underlayer contains the following components by weight percentage: C 0.03~0.08, Si 0.3~0.5, P / s 0.02~0.03, Mn 0.8~1.0, Cr 16~25, Ni 8~12, other alloying elements Mo+V++Ti 0.8~1.5, balance Fe; the hardness of the underlayer is HSD 30~40.

[0026] (2) Preparation of transition layer flux-cored wire: The composition of the transition layer flux-cored wire is prepared according to the composition of the underlayer alloy. The transition layer flux-cored wire contains the following components by weight percentage: C 0.15~0.25, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.0~1.5, Cr 11~13, Ni 2.0~3.0, other alloying elements Mo+V+W 2.0~3.0, balance Fe; transition layer hardness HSD 55~65.

[0027] (3) Preparation of working layer flux-cored wire: The composition of the working layer flux-cored wire is prepared according to the alloy composition of the transition layer. The working layer flux-cored wire contains the following components by weight percentage: C 0.25~0.35, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.2~1.8, Cr 12~15, Mo 2.0~3.0, other alloying elements Ni+V+W 4.0~6.0, and the balance is Fe; the working layer hardness HSD 65~75.

[0028] (4) The flux-cored wire matching experiment requires that the slag be removed cleanly and that elements be burned off as little as possible and silicon be added.

[0029] Step 3: Preheating the rolls (1) Place the roll horizontally on the trolley of the heat treatment furnace and feed it into the furnace smoothly.

[0030] (2) Preheating temperature 500℃, heating rate 20℃ / h, heating time 25 hours, heat preservation 500℃, heat preservation time calculated according to roller diameter / 60, and internal circulation of axial flow fan to maintain uniform temperature.

[0031] Step 4: Pre-welding preparation (1) Drying of welding wire and flux: heat to 300℃ and keep warm for 2 hours.

[0032] (2) Adjust the height of the support roller, hoist the preheated roll onto the welding machine, adjust the position of the heat preservation cover, adjust the speed to 460-550 mm / minute; adjust the position of the machine head, the distance from the machine head to the center line of the roll surface is 15-25 mm, and the welding wire extension is 20-30 mm.

[0033] Step 5: Welding Requirements (1) Process parameters:

[0034] Note: n — number of layers.

[0035] (2) The weld bead should be smooth and free from defects such as porosity, slag inclusion, missing material, hot cracking, and cold cracking.

[0036] (3) The interlayer temperature is maintained at 260-350℃.

[0037] (4) The thickness of a single layer is 4.5 to 6.5 mm. The thickness of the working layer and the weld layer is determined according to the thickness of the wear-resistant layer in the drawing.

[0038] Step 6: Intermediate heat treatment (1) Intermediate heat treatment: When the thickness of the weld layer on one side reaches 20mm, intermediate heat treatment should be adopted to prevent excessive thermal stress.

[0039] (2) Intermediate heat treatment temperature parameters: temperature 520℃, heating rate 20℃ / h, holding time calculated according to roller diameter / 60, cooling rate not greater than 20℃ / h, using axial flow fan internal circulation to maintain uniform temperature, when the temperature drops to 400℃, secondary welding can be performed.

[0040] (3) The number of intermediate heat treatments is determined based on the thickness of the wear-resistant layer.

[0041] Step 7: Final heat treatment Final heat treatment temperature parameters: temperature 520℃, heating rate 20℃ / h, holding time calculated based on roller diameter mm / 60, cooling rate not greater than 20℃ / h, using an axial flow fan for internal circulation to maintain uniform temperature, and the furnace door can only be opened when the temperature drops to below 80℃.

[0042] Step 8: Machining (1) Machin the rolls according to the drawing requirements, with the roll surface diameter being 0.5 mm larger than the standard value.

[0043] (2) Grind to the standard value and surface finish using a grinding machine.

[0044] Step 9: Inspection (1) Perform a hardness test according to the roll standard to repair the roll hardness HSD 65~70.

[0045] (2) Perform ultrasonic testing according to the roll standard.

[0046] Step 10: Packaging; Shipment.

[0047] Example In this embodiment, a high-chromium steel composite vertical roll (E1-E2) from the scrapped 2150 hot continuous rolling mill of Ansteel, with a diameter of 1100mm and roll number AG2016199Y / AG2016202Y, is used as the base material. A repair layer is welded onto the surface of the base material. This repair layer consists of an underlayer, a transition layer, and a working layer, arranged sequentially from the base material surface outwards. In this embodiment, the preparation of the underlayer flux-cored welding wire is based on the alloy composition of the roll. The underlayer flux-cored welding wire contains the following components by weight percentage: C 0.03-0.08, Si 0.3-0.5, P / s 0.02-0.03, Mn 0.8-1.0, Cr 16-25, Ni 8-12, and other alloying elements Mo+V++Ti 0.8-1.5, with the balance being Fe; the hardness of the underlayer is HSD 30-40. The transition layer flux-cored wire is prepared according to the composition of the underlayer alloy. The transition layer flux-cored wire contains the following components by weight percentage: C 0.15~0.25, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.0~1.5, Cr 11~13, Ni 2.0~3.0, other alloying elements Mo+V+W 2.0~3.0, and the balance is Fe; the transition layer hardness HSD 55~65. Preparation of the working layer flux-cored wire: The composition of the working layer flux-cored wire is prepared according to the alloy composition of the transition layer. The working layer flux-cored wire contains the following components by weight percentage: C 0.25~0.35, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.2~1.8, Cr 12~15, Mo 2.0~3.0, other alloying elements Ni+V+W 4.0~6.0, with the balance being Fe; the working layer hardness HSD 65~75.

[0048] The specific method for repairing and remanufacturing this large composite high-chromium steel roll by overlay welding is as follows: Step 1: Roll Preparation (1) Turning of the fatigue layer of the roll: The roll is turned 5mm on one side of the lathe, and the defective parts are cleaned up. (2) The chemical composition of the shavings from the turning part is tested for C, S, P, Mn, Cr, Ni, Mo, V, W and Ti; (3) Ultrasonic testing was performed on the roller surface; Step 2: Welding Material Preparation (1) Preparation of the flux-cored wire for the bottom layer: According to the alloy element composition of the roll, adjust the composition of the flux-cored wire. The bottom layer wire contains the following components by weight percentage: C 0.03~0.08, Si 0.3~0.5, P / s 0.02~0.03, Mn 0.8~1.0, Cr 16~25, Ni 8~12, other alloying elements Mo+V++Ti 0.8~1.5, with the balance being Fe; the bottom layer hardness is HSD35.

[0049] (2) Preparation of transition layer welding wire: According to the alloy element composition of the bottom layer, adjust the composition of the flux-cored welding wire. The transition layer welding wire contains the following components by weight percentage: C 0.15~0.25, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.0~1.5, Cr 11~13, Ni 2.0~3.0, other alloying elements Mo+V+W 2.0~3.0, and the balance is Fe; the hardness of the transition layer is HSD 55.

[0050] (3) Preparation of working layer welding wire: Adjust the composition of flux-cored welding wire according to the alloy element composition of the bottom layer. The working layer welding wire contains the following components by weight percentage: C 0.25~0.35, Si 0.3~0.5, P / s 0.02~0.03, Mn 1.2~1.8, Cr 12~15, Mo 2.0~3.0, other alloying elements Ni+V+W 4.0~6.0, with the balance being Fe; working layer hardness HSD65.

[0051] (4) Welding wire and flux combination experiment: the welding wire and flux combination should be clean and slag removed, and the elements should be burned off as little as possible and the silicon content should be reduced. Step 3: Preheating the rolls (1) Place the roll horizontally on the trolley of the heat treatment furnace and feed it into the furnace smoothly; (2) Preheating temperature 500℃, heating rate 20℃ / h, heating time 25 hours, heat preservation 500℃, heat preservation time calculated according to roller diameter / 60, heat preservation time 18h, and use axial flow fan internal circulation to maintain uniform temperature; Step 4: Pre-welding preparation (1) Dry the welding wire and flux, heat to 300℃, and keep warm for 2 hours; (2) Adjust the height of the support rollers, hoist the preheated rolls onto the welding machine, adjust the position of the heat insulation cover, and adjust the rotation speed to 480 mm / minute. Adjust the position of the die head so that the distance from the die head to the center line of the roll surface is 20 mm, and the wire extension is 25 mm. Step 5: Welding Requirements (1) Process parameters:

[0052] (2) The weld bead should be smooth and free from defects such as porosity, slag inclusion, missing material, hot cracking, and cold cracking; (3) The interlayer temperature should be maintained at 260-350℃. If the temperature cannot be reached, liquefied gas should be used for heating. (4) The thickness of a single layer is 5.0 mm, and the working layer weld layer is determined according to the thickness of the wear-resistant layer 21; Step 6: Intermediate heat treatment (1) Intermediate heat treatment: When the thickness of the weld layer on one side reaches 20mm, intermediate heat treatment should be carried out to prevent excessive thermal stress. (2) Intermediate heat treatment temperature parameters: temperature 520℃, heating rate 20℃ / h, heating time 24h, holding time calculated according to roller diameter / 60, holding time 18h, cooling rate not greater than 20℃ / h, using axial flow fan internal circulation to maintain uniform temperature, when the temperature drops to 400℃, secondary welding can be carried out. (3) The number of intermediate heat treatments is determined to be 5 times based on the thickness of the wear-resistant layer; Step 7: Final heat treatment Final heat treatment temperature parameters: temperature 520℃, heating rate 20℃ / h, heating time 18h, holding time calculated based on roller diameter mm / 60, holding time 20h, cooling rate not greater than 20℃ / h, using axial flow fan for internal circulation to maintain uniform temperature, the furnace door can only be opened when the temperature drops to below 80℃. Step 8: Machining (1) Machin the rolls according to the drawings, with the roll diameter being 0.5 mm larger than the standard value; (2) Grind the rolls to the standard value and surface finish using a grinding machine; Step 9: Inspection (1) Perform a hardness test of 65-70 HSD according to the roll standard; (2) Perform ultrasonic flaw detection tests according to the roll standard; Step 10: Packaging. Shipped from factory. (1) Remove rust from the rolls, polish and oil them; (2) Wrap the roller surface with plastic sheeting, support the roller surface with wooden support, and wrap it securely with packaging straps; (3) Product warranty certificate.

[0053] Field usage report of large composite high-chromium steel rolls repaired and remanufactured by overlay welding: (1) 2150 hot rolling mill roll usage record

[0054]

[0055]

[0056] (2) On-site usage report 2150 hot rolling mill weld overlay rolls: Roll number AG2016199Y / AG2016202Y usage status.

[0057] It has been tested four times and is still in use. The surface is excellent, and there have been no quality problems with the strip edges caused by poor vertical roll surface. The surface is smooth and has a certain degree of wear resistance. A comparison of actual machine data clearly shows that the rolling performance of this pair of welded rolls is significantly better than that of all other vertical rolls made of currently used materials. The price is also competitive, with a cost per ton of steel only about 40% of that of high-chromium cast steel combined vertical rolls, and its wear resistance is second only to high-chromium cast steel, receiving high praise from the user.

[0058] Although this application has been described above with reference to specific embodiments, those skilled in the art will understand that many modifications can be made to the configurations and details disclosed in this application within the principles and scope of the disclosure. The scope of protection of this application is determined by the appended claims, and the claims are intended to cover all modifications included in the literal meaning or scope of equivalents of the technical features in the claims.

Claims

1. A reconstructed layer for welding repair of large composite high-carbon high-chromium steel rolls, characterized in that: The system comprises a base surface, a base layer, a transition layer, and a working layer, connected sequentially. The base layer is formed by welding with a base layer flux-cored wire, the transition layer by welding with a transition layer flux-cored wire, and the working layer by welding with a working layer flux-cored wire. The base layer flux-cored wire is composed of the following components by weight percentage: C 0.03–0.08, Si 0.3–0.5, P 0.02–0.03, S 0.02–0.03, Mn 0.8–1.0, Cr 16–25, Ni 8–12, and alloying elements Mo+V+Ti 0.8–1.5, with the balance being Fe. The transition layer flux-cored wire is composed of the following components by weight percentage: C 0.15–0.25, Si 0.3–0.5, P 0.02–0.03, S 0.02–0.03, Mn 1.0–1.5, Cr The working layer flux-cored wire is composed of the following components by weight percentage: C 0.25-0.35, Si 0.3-0.5, P 0.02-0.03, S 0.02-0.03, Mn 1.2-1.8, Cr 12-15, Mo 2.0-3.0, Ni+V+W 4.0-6.0, with the balance being Fe. The hardness HSD of the underlayer is 30-40, the hardness HSD of the transition layer is 55-65, and the hardness HSD of the working layer is 65-75.

2. The large composite high-carbon high-chromium steel roll overlay repair and remanufacturing layer as described in claim 1, characterized in that: The base layer consists of 2 layers, the transition layer consists of 2 layers, and the working layer consists of several layers.

3. A method for preparing a reconstructed layer for welding repair of large composite high-carbon high-chromium steel rolls as described in any one of claims 1 to 2, characterized in that: The method includes preheating the roll, placing the preheated roll on a welding machine, welding the bottom layer flux-cored wire on the preheated roll in proportion to form the bottom layer, welding the transition layer flux-cored wire on the bottom layer in proportion to form the transition layer, welding the working layer flux-cored wire on the transition layer in proportion to form the working layer, performing intermediate heat treatment when the thickness of the weld layer on one side reaches 20-30mm, performing final heat treatment after the welding is completed, and grinding the roll after the final heat treatment to complete the repair and reconstruction of the roll.

4. The method as described in claim 3, characterized in that: The preheating temperature is 500℃, the heating rate is 20℃ / h, the heating time is 25 hours, and the temperature is maintained at 500℃. The holding time is calculated based on the roller diameter in mm / 60. An axial flow fan is used for internal circulation to maintain uniform temperature.

5. The method as described in claim 3, characterized in that: The intermediate heat treatment temperature is 520℃, the heating rate is 20℃ / h, the holding time is calculated based on the roller diameter mm / 60, the cooling rate is no more than 20℃ / h, and an axial flow fan is used for internal circulation to maintain uniform temperature. When the temperature drops to 400℃, a secondary welding is performed.

6. The method according to any one of claims 3 to 5, characterized in that: The final heat treatment temperature is 520℃, the heating rate is 20℃ / h, the holding time is calculated based on the roller diameter (mm / 60), the cooling rate is no more than 20℃ / h, and an axial flow fan is used for internal circulation to maintain uniform temperature. The furnace door is opened when the temperature drops to below 80℃.

7. The method as described in claim 6, characterized in that: The interlayer temperature of each working layer is 260-350℃, the interlayer temperature of each base layer is 260-350℃, and the interlayer temperature between adjacent working layers and base layers is 260-350℃.

8. The method as described in claim 6, characterized in that: The thickness of the working layer or the base layer is 4.5 to 6.5 mm.

Citation Information

Patent Citations

  • Surfacing reconstructed layer of large hot-rolled supporting roll Cr4 and method for repairing roll

    CN105436665A

  • Overlaying rebuilt layer for large cold-rolled supporting roll 70 Cr3Mo and method for repairing roll

    CN105478962A

  • Wear-resistant grinding roller

    CN112547224A