Method for controlling silicon and phosphorus concentrations in carbonated leach solution of vanadium-containing clinker
By using magnesium bicarbonate as an inhibitor in the vanadium extraction process of vanadium slag calcination-calcination-carbonation leaching, the leaching problem of silicon and phosphorus impurities was solved, achieving effective removal under alkaline conditions and recycling of process water, thus reducing costs and investment.
Patent Information
- Application Number
- CN202311609787.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-27
AI Technical Summary
In the vanadium slag calcination-calcination-carbonation leaching process, existing technologies struggle to effectively suppress the leaching of silicon and phosphorus impurities under alkaline conditions without affecting the recycling of process water.
Magnesium bicarbonate is used as an inhibitor. It reacts with NH⁴⁺ and PO₄³⁻ in the leachate to form insoluble magnesium ammonium phosphate precipitate, and reacts with silicon to form magnesium silicate precipitate. Excess magnesium bicarbonate is converted into slightly soluble magnesium carbonate, avoiding the introduction of anions that affect the process water circulation. Vanadate and magnesium ions react to form water-soluble magnesium vanadate, reducing vanadium loss.
It enables the suppression of silicon and phosphorus impurities under alkaline conditions, reduces process costs and engineering investment, avoids the need for a dedicated leaching solution impurity removal process, and ensures the recycling of process water.
Smart Images

Figure CN117737463B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of vanadium extraction and metallurgical technology, specifically relating to a method for controlling the concentration of silicon and phosphorus in the carbonation leaching solution of vanadium-containing clinker. Background Technology
[0002] Vanadium slag is the main raw material for producing vanadium oxide, and the traditional industrial process is sodium roasting followed by water leaching for vanadium extraction. This process involves a large amount of sodium carbonate as a roasting additive and high water treatment costs, resulting in high vanadium oxide production costs. Furthermore, the treatment of vanadium precipitation wastewater generates a large amount of difficult-to-treat vanadium-chromium filter cake and sodium sulfate, posing significant environmental risks. To address the problems of high production costs and significant environmental risks associated with existing vanadium oxide production, a process of vanadium slag calcification roasting followed by carbonation leaching for vanadium extraction is proposed. The specific process can be found in invention patent application CN110106344A. During the carbonation leaching process of vanadium-containing clinker, a small amount of silicon and phosphorus dissolves into the leaching solution, which is detrimental to the preparation of high-quality vanadium oxide.
[0003] In the field of vanadium hydrometallurgy, there are mature technologies for removing silicon and phosphorus from alkaline solutions. Generally, aluminum sulfate is used for silicon removal and calcium chloride for phosphorus removal, which can reduce the concentration of silicon and phosphorus in alkaline vanadium-containing solutions to below 0.01 g / L. However, because the above two reagents introduce sulfate and chloride ions into the solution system, they cannot meet the technical requirements for the recycling of process water in the vanadium slag calcination-carbonation leaching vanadium extraction process.
[0004] To address the issue of simultaneous removal of silicon and phosphorus from alkaline vanadium-containing solutions, patent application CN112095025A proposes a method for removing silicon and phosphorus from a blank roasting-ammonia leaching vanadium solution. This method involves adjusting the pH of the leachate to 7–7.3, adding polyacrylamide for flocculation and sedimentation, and then precision filtration to obtain a leachate with low silicon and phosphorus concentrations. However, this method requires controlling the pH of the leachate to be low and within a narrow range. Since the pH of the carbonated leachate is approximately 9.5, adjusting it to pH 7–7.3 will result in carbonate decomposition and sodium bicarbonate crystallization, increasing the complexity of the process and affecting media circulation. The published literature "Research on Comprehensive Utilization of High-Chromium Vanadium Slag" uses ammonium sulfate and magnesium sulfate to remove impurities such as silicon and phosphorus from alkaline vanadium-chromium solutions. This method can reduce the silicon and phosphorus concentrations to below 0.02 g / L, but the introduction of sulfate ions by the impurity removal reagents will affect the recycling of water in the vanadium slag calcination-roasting-carbonation leaching process. Patent application CN104843789A provides a method for purifying vanadium pentoxide. By adding aluminum sulfate to the alkaline leaching solution to simultaneously remove silicon and phosphorus impurities, the introduction of sulfate ions into the impurity removal reagent will affect the recycling of water in the vanadium slag calcination-carbonation leaching process.
[0005] Patent application CN101724756A discloses a method for removing phosphorus and silicon from vanadium-containing clinker leachate: The method involves setting the temperature of the vanadium-containing clinker leachate within the range of 60°C to boiling; adjusting the pH value of the vanadium-containing clinker leachate; adjusting the pH value of the vanadium-containing clinker leachate using acid and alkali according to the type of purifying agent to be added; adding the purifying agent, the amount of which is determined based on the amount of phosphorus and silicon detected in the vanadium-containing clinker leachate and the reaction formula between the phosphorus and silicon in the vanadium-containing clinker leachate and the purifying agent; cooling and filtering the resulting vanadium-containing clinker leachate to obtain a low-phosphorus, low-silicon vanadium solution. The purifying agent used can be a substance selected from aluminum salts, iron salts, magnesium salts, and groups thereof. Aluminum salts can be aluminum sulfate, aluminum chloride, and aluminum nitrate; iron salts can be ferric sulfate, ferric chloride, and ferric nitrate; magnesium salts can be magnesium sulfate, magnesium chloride, and magnesium nitrate. However, the sulfate, chloride, and nitrate ions introduced by the added purifying agent can affect the recycling of process water.
[0006] Therefore, under alkaline conditions, the technical problem of how to suppress the leaching of silicon and phosphorus impurities, or remove silicon and phosphorus impurities from the carbonation leachate, without affecting the recycling of process water, still needs to be solved. At present, there are no reports of relevant technologies that can effectively solve the above problems and have industrial application prospects. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention proposes a method for controlling the concentration of silicon and phosphorus in the carbonation leaching solution of vanadium-containing clinker. This method can at least suppress the leaching of silicon and phosphorus impurities under alkaline conditions, or remove silicon and phosphorus impurities from the carbonation leaching solution, without affecting the recycling of process water.
[0008] The present invention provides a method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker, comprising the following steps:
[0009] a. A leaching slurry is formed by mixing vanadium-containing clinker and vanadium precipitation supernatant. Inhibitors controlling silicon and phosphorus leaching are added to the leaching slurry to initiate the leaching reaction. The main vanadium-containing phases in the vanadium-containing clinker are calcium vanadate and manganese vanadate. The vanadium-containing clinker is leached using the vanadium precipitation supernatant. Because the supernatant contains a large amount of carbonate and bicarbonate ions, and calcium and manganese carbonates have lower solubility than vanadates, calcium vanadate and manganese vanadate are converted into calcium carbonate and manganese carbonate, which have even lower solubility, allowing vanadium to dissolve into the leaching solution.
[0010] b. After the leaching reaction is completed, solid and liquid are separated to obtain leachate and leaching residue;
[0011] In step a, the inhibitor is magnesium bicarbonate. The purpose of choosing magnesium bicarbonate as a reagent to remove silicon and phosphorus is twofold: firstly, to reduce the added Mg... 2+ With NH in the leachate 4+ PO4 3-The reaction forms a sparingly soluble magnesium ammonium phosphate precipitate, which reacts with silicon to form magnesium silicate precipitate, thus achieving the removal of silicon and phosphorus. Secondly, excess magnesium bicarbonate is converted into slightly soluble magnesium carbonate during leaching, avoiding the introduction of anions that could affect the process water circulation and preventing high magnesium concentration in the leachate due to excessive magnesium salt addition. Thirdly, the magnesium vanadate formed by the reaction of vanadate and magnesium ions is water-soluble, avoiding vanadium loss due to the introduction of impurity removal reagents. Specifically, the chemical reaction equation for the removal of silicon and phosphorus using magnesium bicarbonate reagent is PO4⁻. 3- +NH4 + +Mg 2+ =MgNH4PO4↓; SiO3 2- +Mg 2+ =MgSiO3↓; The chemical reaction equation for the conversion of magnesium bicarbonate into slightly soluble magnesium carbonate during leaching is Mg(HCO3)2=MgCO3↓+CO2↑+H2O.
[0012] Furthermore, in step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added to the immersion mixing tank for further pulping to form the leaching slurry, making the leaching slurry more uniformly mixed.
[0013] Furthermore, in step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added to the leaching tank, then heated to 90–95°C. On the one hand, at this temperature, silicon and phosphorus have fully dissolved into the leaching solution, allowing them to precipitate into the leaching residue, effectively controlling the concentration of silicon and phosphorus in the leaching solution. On the other hand, the leaching slurry is leached at high temperatures for a shorter time, resulting in less decomposition of ammonium carbonate and ammonium bicarbonate in the supernatant, meaning a higher ammonia concentration in the leaching solution, which is beneficial for magnesium bicarbonate phosphorus removal.
[0014] Furthermore, in step a, the leaching reaction is kept at a constant temperature for 1 to 2 hours to ensure that the leaching reaction proceeds fully.
[0015] Furthermore, in step a, the vanadium-containing clinker is either a blank vanadium slag or a product of calcification roasting, and the main vanadium-containing phases of the vanadium-containing clinker are calcium vanadate and manganese vanadate.
[0016] Furthermore, in step a, the vanadium precipitation supernatant is a carbonation leaching solution obtained by precipitating vanadium with ammonium bicarbonate and / or ammonium carbonate.
[0017] Furthermore, in step a, the amount of magnesium bicarbonate used is 1.8% to 2.5% of the weight of the vanadium-containing clinker.
[0018] Furthermore, the leaching reaction is carried out at a pH between 9 and 10.
[0019] Furthermore, the leachate produced in step b can be directly used to precipitate ammonium metavanadate.
[0020] Furthermore, the heating in step a is carried out using a water bath.
[0021] The beneficial effects of this invention are as follows: This invention utilizes magnesium bicarbonate to simultaneously remove silicon and phosphorus impurities. Excess magnesium bicarbonate is converted into magnesium carbonate precipitate during the carbonation leaching process of clinker, without introducing harmful ions that affect the recycling of process water. Furthermore, it inhibits the leaching of silicon and phosphorus during the carbonation leaching process of vanadium-containing clinker, eliminating the need for a dedicated leaching solution impurity removal process, thereby reducing process costs and engineering investment. Attached Figure Description
[0022] Figure 1 The diagram shows a process flow chart of a method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker provided by the present invention. Detailed Implementation
[0023] It should be understood that the embodiments of the invention shown in the exemplary embodiments are merely illustrative. Although only a few embodiments have been described in detail in this invention, those skilled in the art will readily recognize that various modifications are possible without substantially departing from the teachings of the invention. Accordingly, all such modifications should be included within the scope of the invention. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention.
[0024] This invention provides a method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker, such as... Figure 1 As shown, it includes the following steps:
[0025] a. A leaching slurry is formed by mixing vanadium-containing clinker and vanadium precipitation supernatant. Inhibitors controlling silicon and phosphorus leaching are added to the leaching slurry to initiate the leaching reaction. The main vanadium-containing phases in the vanadium-containing clinker are calcium vanadate and manganese vanadate. The vanadium-containing clinker is leached using the vanadium precipitation supernatant. Because the supernatant contains a large amount of carbonate and bicarbonate ions, and calcium and manganese carbonates have lower solubility than vanadates, calcium vanadate and manganese vanadate are converted into calcium carbonate and manganese carbonate, which have even lower solubility, allowing vanadium to dissolve into the leaching solution.
[0026] b. After the leaching reaction is completed, solid and liquid are separated to obtain leachate and leaching residue;
[0027] In step a, the inhibitor is magnesium bicarbonate.
[0028] This invention utilizes magnesium bicarbonate to simultaneously remove silicon and phosphorus impurities. Excess magnesium bicarbonate is converted into magnesium carbonate precipitate during the carbonation leaching process of clinker, without introducing harmful ions that affect the recycling of process water. Furthermore, it inhibits the leaching of silicon and phosphorus during the carbonation leaching process of vanadium-containing clinker, eliminating the need for a dedicated leaching solution impurity removal process, thus reducing process costs and engineering investment. Specifically, magnesium bicarbonate is chosen as the reagent for removing silicon and phosphorus, firstly because of the added Mg... 2+With NH in the leachate 4+ PO4 3- The reaction forms a sparingly soluble magnesium ammonium phosphate precipitate, which reacts with silicon to form magnesium silicate precipitate, thus achieving the removal of silicon and phosphorus. Secondly, excess magnesium bicarbonate is converted into slightly soluble magnesium carbonate during leaching, avoiding the introduction of anions that could affect the process water circulation and preventing high magnesium concentration in the leachate due to excessive magnesium salt addition. Thirdly, the magnesium vanadate formed by the reaction of vanadate and magnesium ions is water-soluble, avoiding vanadium loss due to the introduction of impurity removal reagents. Specifically, the chemical reaction equation for the removal of silicon and phosphorus using magnesium bicarbonate reagent is PO4⁻. 3- +NH4 + +Mg 2+ =MgNH4PO4↓; SiO3 2- +Mg 2+ =MgSiO3↓; The chemical reaction equation for the conversion of magnesium bicarbonate into slightly soluble magnesium carbonate during leaching is Mg(HCO3)2=MgCO3↓+CO2↑+H2O.
[0029] In some embodiments, in step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added to an immersion mixing tank for further pulping to form the leaching slurry, thereby making the leaching slurry more uniformly mixed.
[0030] In some embodiments, in step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added to the leaching tank, and then heated to 90-95°C. On the one hand, at this temperature, silicon and phosphorus have fully dissolved into the leaching solution, allowing the silicon and phosphorus in the leaching solution to precipitate into the leaching residue, effectively controlling the concentration of silicon and phosphorus in the leaching solution. On the other hand, the leaching slurry is leached at high temperatures for a shorter time, resulting in less decomposition of ammonium carbonate and ammonium bicarbonate in the supernatant, meaning a higher ammonia concentration in the leaching solution, which is beneficial for magnesium bicarbonate phosphorus removal.
[0031] In some embodiments, in step a, the leaching reaction is kept at a constant temperature for 1 to 2 hours to ensure the leaching reaction proceeds fully.
[0032] In some embodiments, in step a, the vanadium-containing clinker is either a blank vanadium slag or a product of calcification roasting. The main vanadium-containing phases of the vanadium-containing clinker are calcium vanadate and manganese vanadate.
[0033] In some embodiments, in step a, the vanadium precipitation supernatant is a solution obtained by precipitating vanadium using ammonium bicarbonate and / or ammonium carbonate from a carbonation leaching solution.
[0034] In some embodiments, in step a, the amount of magnesium bicarbonate used is 1.8% to 2.5% of the weight of the vanadium-containing clinker.
[0035] In some embodiments, the leaching reaction is carried out at a pH between 9 and 10, which is more suitable for the alkaline environment of the carbonation leachate.
[0036] In some embodiments, the leachate produced in step b can be used directly to precipitate ammonium metavanadate.
[0037] In some embodiments, the heating in step a is performed using a water bath.
[0038] The present invention will be further described in detail below through specific embodiments and comparative examples.
[0039] Example 1
[0040] 500g of vanadium-containing clinker (TV 7.10%, P 0.06%, SiO2 14.91%) was mixed with 1000mL of vanadium precipitation supernatant (NH4). + 28.35 g / L, CO3 2- 21.25 g / L, HCO 3- The sample (134.25 g / L, TV 5.94 g / L, pH 9.09) was pulped, heated to 92℃ in a water bath, and 10 g of magnesium bicarbonate was added. The leaching reaction was carried out at a constant temperature for 120 min. After the leaching reaction was completed, the solid and liquid were separated, and the chemical composition of the obtained leachate was TV 38.38 g / L, Si 0.03 g / L, and P 0.02 g / L.
[0041] Example 2
[0042] 500g of vanadium-containing clinker (TV 7.10%, P 0.06%, SiO2 14.91%) was mixed with 1000mL of vanadium precipitation supernatant (NH4). + 28.35 g / L, CO3 2- 21.25 g / L, HCO 3- The sample (134.25 g / L, TV 5.94 g / L, pH 9.09) was pulped, heated to 92℃ in a water bath, and 11 g of magnesium bicarbonate was added. The leaching reaction was carried out at a constant temperature for 120 min. After the leaching reaction was completed, the solid and liquid were separated, and the chemical composition of the obtained leachate was TV 38.24 g / L, Si 0.02 g / L, and P 0.02 g / L.
[0043] Example 3
[0044] 500g of vanadium-containing clinker (TV 7.10%, P 0.06%, SiO2 14.91%) was mixed with 1000mL of vanadium precipitation supernatant (NH4). + 28.35 g / L, CO3 2- 21.25 g / L, HCO 3- The sample (134.25 g / L, TV 5.94 g / L, pH 9.09) was pulped, heated to 92℃ in a water bath, and 12.5 g of magnesium bicarbonate was added. The leaching reaction was carried out at a constant temperature for 120 min. After the leaching reaction was completed, the solid and liquid were separated, and the chemical composition of the obtained leachate was TV 38.47 g / L, Si 0.02 g / L, and P 0.01 g / L.
[0045] Comparative Example
[0046] 500g of vanadium-containing clinker (TV 7.10%, P 0.06%, SiO2 14.91%) was mixed with 1000mL of vanadium precipitation supernatant (NH4). + 28.35 g / L, CO3 2- 21.25 g / L, HCO 3- The sample was pulped (134.25 g / L, TV 5.94 g / L, pH 9.09), heated in a water bath to 92℃, and leached for 120 min at a constant temperature. After the leaching reaction, the solid and liquid were separated, and the chemical composition of the leachate was TV 38.32 g / L, Si 0.26 g / L, and P 0.15 g / L.
[0047] In summary, using magnesium bicarbonate as an inhibitor in the leaching reaction results in lower silicon and phosphorus content in the leachate, better impurity removal, and eliminates the need for a dedicated leachate impurity removal process, thereby reducing process costs and engineering investment.
[0048] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the present invention. Any modifications or equivalent substitutions made to the present invention without departing from the spirit and scope thereof should be covered within the protection scope of the claims of the present invention.
Claims
1. A method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker, characterized in that, Includes the following steps: a. Mix vanadium-containing clinker and vanadium precipitation supernatant to form a leaching slurry. Add inhibitors to the leaching slurry to control the leaching of silicon and phosphorus to carry out the leaching reaction. The vanadium precipitation supernatant is a carbonation leaching solution using ammonium bicarbonate and / or ammonium carbonate after vanadium precipitation. b. After the leaching reaction is completed, solid and liquid are separated to obtain leachate and leaching residue; In step a, the inhibitor is magnesium bicarbonate.
2. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, In step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added to an immersion mixing tank for further pulping to form the leaching slurry.
3. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, In step a, the vanadium-containing clinker and the vanadium-precipitated supernatant are mixed and added into an immersion mixing tank, and then heated to 90-95°C.
4. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 3, characterized in that, In step a, the leaching reaction is kept at a constant temperature for 1 to 2 hours.
5. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, In step a, the vanadium-containing clinker is either a blank vanadium slag or a product of calcification roasting.
6. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, In step a, the amount of magnesium bicarbonate used is 1.8% to 2.5% of the weight of the vanadium-containing clinker.
7. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, The leaching reaction is carried out at a pH between 9 and 10.
8. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 1, characterized in that, The leachate produced in step b can be directly used to precipitate ammonium metavanadate.
9. The method for controlling the silicon and phosphorus concentrations in the carbonation leaching solution of vanadium-containing clinker according to claim 3, characterized in that, In step a, the temperature is increased using a water bath.
Citation Information
Patent Citations
Method for purifying vanadium pentoxide
CN104843789A
Method for removing silicon and phosphorus from blank roasting-ammonia leaching vanadium extracting solution
CN112095025A
Phosphorus and silicon removing method of vanadium-contained clinker leaching liquor
CN101724756A
Method for purifying vanadium leaching solution
CN102251113A
Process for separating and purifying molybdenum in low-molybdenum-content tailings
CN103343244A