A tin-antimony-nickel dimensionally stable electrode prepared based on electroplating and dipping method, and a preparation method and application thereof

Tin-antimony-nickel electrodes were prepared by electroplating and impregnation methods, which solved the problems of low stability and Faraday efficiency of existing electrocatalysts, and achieved efficient, stable and low-cost ozone preparation, which is suitable for electrochemical oxidation reactions.

CN117737773BActive Publication Date: 2026-11-24ZHEJIANG UNIV OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311470889.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-07
Publication Date
2026-11-24
Estimated Expiration
2043-11-07

AI Technical Summary

Technical Problem

Existing electrocatalyst materials for ozone generation suffer from insufficient stability, low Faraday efficiency, and high cost. In particular, PbO₂ and Ni-Sb-SnO₂ have problems with pollution and high production costs in long-term use.

Method used

Tin-antimony-nickel electrodes were prepared by electroplating and impregnation. Sn and Sb were electrodeposited on a titanium sheet to form SnO₂ and Sb₂O₃ coatings, and then impregnated in a nickel salt solution to form an impregnation-Ni-Sb-SnO₂-Ti electrode, which improved the stability and activity of the catalyst.

Benefits of technology

The prepared tin-antimony-nickel electrode exhibits high catalytic efficiency and good stability in the electrocatalytic preparation of ozone, with a Faraday efficiency of up to 48%, and is pollution-free. The preparation process is simple and has low energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117737773B_ABST
    Figure CN117737773B_ABST
Patent Text Reader

Abstract

This invention discloses a tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation methods, its preparation method, and its application. The electrode preparation method involves: preparing an electrodeposition solution containing stannous salt and trivalent antimony salt; using a pretreated titanium sheet as the cathode; inserting the anode and cathode into the electrodeposition solution; connecting the anode and cathode to the positive and negative terminals of a power source, respectively; depositing Sn and Sb through an electrolytic reaction; then performing a first calcination treatment in a muffle furnace; immersing the calcined titanium sheet in a nickel salt solution for impregnation; drying; and performing a second calcination treatment in a muffle furnace to obtain the final size-stabilized electrode. The catalyst, support, and active components of this invention are widely available, low in toxicity, require no precious metals, exhibit excellent electrocatalytic ozone production performance and electrocatalytic stability, and possess good overall mechanical properties, are pollution-free, and are easy to prepare, showing great application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials preparation technology, specifically relating to a tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation methods, its preparation method, and its application. Background Technology

[0002] Ozone (O3) is one of the most important oxides in daily life and chemical industry, widely used in disinfection, papermaking, chemical synthesis, and wastewater treatment. Current ozone production processes are mainly based on the high-voltage corona discharge method, which generates high concentrations of ozone but also results in high energy consumption and large amounts of nitrogen oxides, which are carcinogenic to humans. Furthermore, the instability and strong corrosiveness of ozone pose safety concerns during transportation and storage. In practical applications, most ozone applications require dilution, and ozone exhaust gases need to be specifically decomposed. To enable on-demand, distributed ozone production using renewable electricity, the electrochemical ozone generation (EOP) pathway has emerged as a promising alternative. The key to large-scale implementation of this pathway is the development of highly selective, active, and economical electrocatalysts.

[0003] PbO2, Ni-Sb-SnO2, and boron-doped diamond (BDD) have long been studied as electrocatalysts for ozone production (EOP). However, PbO2 causes Pb dissolution during long-term use, leading to water pollution. BDD's application is limited due to its high production cost. Ni-Sb-SnO2, using metal oxides as both the support and active component, is readily available and simple to prepare, and does not produce harmful substances during long-term use, making it an excellent catalyst choice. However, its stability and Faraday efficiency can be further improved. By changing the preparation method, using SnO2 as the support, and increasing the surface Ni active component, high concentrations of ozone can be obtained at the anode. After simple treatment, it can be used for sterilization and disinfection. This method of ozone production is scalable, easy to control, and safe and reliable. Summary of the Invention

[0004] To address the aforementioned technical problems in the existing technology, the present invention aims to provide a tin-antimony-nickel size-stable electrode prepared by electroplating and impregnation methods, its preparation method, and its application. The electrocatalyst of the present invention has the advantages of high catalytic efficiency, simple preparation, and high stability. The catalyst of the present invention has widely available sources of support and active components, low toxicity, and does not require the use of precious metals. It has good electrocatalytic ozone preparation performance and electrocatalytic stability. At the same time, its overall mechanical properties are good, it is pollution-free, easy to prepare, and has great application potential.

[0005] The technical solution adopted in this invention is as follows:

[0006] A method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation includes the following steps:

[0007] 1) The titanium sheet is polished to remove the oxide layer on its surface and roughen the surface. Then it is washed and dried to obtain a pretreated titanium sheet.

[0008] 2) Then, an electrodeposition solution containing stannous salt and trivalent antimony salt is prepared. The pretreated titanium sheet is used as the cathode. The anode and cathode are inserted into the electrodeposition solution and connected to the positive and negative terminals of the power supply, respectively. Sn and Sb are electrodeposited on the titanium sheet through an electrolytic reaction. After that, the titanium sheet with Sn and Sb electrodeposited is taken out, dried, and placed in a muffle furnace for a single calcination treatment in air environment to oxidize Sn and Sb to SnO2 and Sb2O3, respectively, to obtain a precipitated-Sb-SnO2 electrode.

[0009] 3) Subsequently, the immersion-Sb-SnO2 electrode was immersed in a nickel salt solution for impregnation treatment. After that, the electrode was taken out and dried, and then placed in a muffle furnace for a second calcination treatment in air environment to oxidize the nickel on the electrode to the oxidized state, thus obtaining the immersion-Ni-Sb-SnO2-Ti electrode, which is now complete.

[0010] Further, the washing in step 1) consists of sequential alkaline washing for degreasing and acid washing for etching. The alkaline washing solution is a NaOH solution with a concentration of 10-40 wt%, preferably 20 wt%, the alkaline washing temperature is 60-100℃, preferably 75-80℃, and the alkaline washing time is 0.5h-3h, preferably 1h. The acid washing solution is an oxalic acid solution with a mass concentration of 5%-20%, preferably 10%, the acid washing etching time is 0.5-4h, preferably 2h, and the acid washing temperature is 60-100℃, preferably 90-95℃.

[0011] Further, in step 2), the solvent for the electrodeposition solution is prepared by mixing choline chloride and ethylene glycol, heating and dissolving them into a colorless and transparent solution. The heating temperature is 60-90℃, preferably 80℃, and the molar ratio of choline chloride to ethylene glycol is 1:1-1:5, preferably 1:2-3.

[0012] Further, in the electrodeposition solution of step 2), the concentration of stannous salt is 0.1-1M, preferably 0.2-0.3M, and the concentration of trivalent antimony salt is 0.005-0.1M, preferably 0.008-0.01M.

[0013] Furthermore, in step 2), when installing the cathode and anode, the titanium sheet is inserted into the middle of the solution as the cathode, and two graphite plates are placed parallel to the cathode as the anode. When viewed at eye level, the titanium sheet is not exposed to the line of sight, so that the graphite plates completely cover the titanium sheet.

[0014] Furthermore, the cathode and anode are installed. A 2*2cm processed titanium sheet is placed in the middle of the solution as the cathode, and two graphite plates are placed parallel to the cathode as the anode. The size of the graphite plates is 2.5*2.5cm-4*4cm, preferably 3*3cm, to ensure that the graphite plates and the titanium sheet are parallel and that the titanium sheet is not exposed in the line of sight when viewed at eye level, so that the graphite plates completely cover the titanium sheet.

[0015] Furthermore, the anode and cathode are connected to the positive and negative electrodes respectively, and a corresponding current is set according to the cathode area. Electrodeposition is performed after a period of time, with a current density of 5-20 mA / cm². 2 Preferably 10 mA / cm 2 The electrodeposition time is 5-40 min, preferably 20 min.

[0016] Further, in step 2), the dried titanium sheet is placed in a muffle furnace for calcination at a temperature of 450℃-700℃, preferably 600℃, for a time of 1-4h, preferably 2h. The size-stable electrode obtained after calcination is named: precipitated-Sb-SnO2-Ti.

[0017] Further, in step 3), the calcined and cooled Sb-SnO2-Ti electrode is immersed in a nickel salt solution of a certain concentration. The nickel salt is nickel chloride hexahydrate, nickel nitrate, or nickel acetate. Nickel acetate is preferred, and the concentration is 0.05-0.5M, preferably 0.1M. The immersion time is 2-12h, preferably 8h.

[0018] Further, in step 3), the impregnated Ni-Sb-SnO2-Ti is placed in a muffle furnace for secondary calcination at a temperature of 450-700℃, preferably 500℃, for a calcination time of 1-4h, preferably 2h. The resulting size-stable electrode is named Ni-Sb-SnO2-Ti.

[0019] The electrocatalyst prepared according to the method of the present invention is composed of titanium sheets and oxides, with SnO2 and Sb2O3 as supports and Ni oxide as the active component.

[0020] The application of the impregnated Ni-Sb-SnO2-Ti size-stabilized electrode in the electrocatalytic preparation of ozone involves using a galvanometer as the electrochemical generating device, employing a two-electrode system, with the impregnated Ni-Sb-SnO2-Ti size-stabilized electrode as the anode, a platinum sheet as the counter electrode, and sulfuric acid solution as the electrolyte to carry out an electrochemical oxidation reaction. The generated ozone gas is detected by a 2Btech instrument, wherein the concentration of the sulfuric acid solution is 0.05-1M, preferably 0.5M.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] 1) This invention provides a method for preparing a tin-antimony-nickel size-stable electrode based on electroplating and impregnation and applying it to prepare ozone with high performance. The titanium sheet processing method is simple, the catalyst preparation process is short and energy consumption is low, the precursor salt is easy to obtain, SnO2 can cover the titanium sheet surface well, the surface is free of cracks and generates a large number of protrusions on the surface, increasing the catalytic area and improving the catalytic efficiency, thus having good catalytic performance.

[0023] 2) In the preparation process of the electrocatalyst of this invention, the titanium sheet serving as the cathode does not undergo hydrogen evolution reaction in the organic phase electrodeposition solution system. Sn and Sb can be well coated on the titanium sheet substrate, and then SnO2 and Sb2O3 are formed by high-temperature oxidation in air. These two substances form an ATO coating with good conductivity. Then, the size-stabilized electrode is immersed in a nickel acetate solution. The nickel acetate penetrates into the interior of the coating, and the acetate macromolecules are embedded in the interlayer gaps on the coating surface, increasing the surface nickel content. During sintering, carbothermic reduction ensures that the nickel is not completely oxidized to trivalent nickel, thus maintaining the high activity of nickel. Finally, a size-stabilized electrode with high ozone activity and high conductivity is obtained.

[0024] 3) The catalyst of this invention, after testing with an electrochemical workstation, a constant current instrument and 2B Tech, has good catalytic effect under acidic conditions, with an ozone production of 400 ppm and a Faraday efficiency of up to 48%. It also has good electrocatalytic ozone stability and has great development potential. Attached Figure Description

[0025] Figure 1 The results show the comparison of the electrocatalytic ozone production performance of the catalysts in Examples 1-5 of this invention;

[0026] Figure 2 Comparison of the gaseous ozone Faraday efficiency of the electrocatalytic ozone preparation reaction of the catalysts in Examples 1-5 of this invention;

[0027] Figure 3 This presents a comparison of the ozone production performance of each catalyst when the catalysts in Comparative Examples 1-7 are used in the electrocatalytic reaction of this invention.

[0028] Figure 4 This is a comparison of the lifetime test (voltage U-time t) results of the electrode catalysts of Example 1 and Comparative Example 1 in the application of electrocatalytic ozone production. Detailed Implementation

[0029] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.

[0030] Example 1

[0031] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0032] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0033] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride and 78 mg of antimony trichloride to the deposition solution and stir to dissolve.

[0034] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0035] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition reaction was carried out for 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140℃.

[0036] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Sb-SnO2-Ti.

[0037] 6) The obtained precipitated Sb-SnO2-Ti electrode was immersed in 50 mL of 0.1 M nickel acetate solution for 8 h, dried, and calcined in a muffle furnace at 500 °C for 2 h to obtain the precipitated Ni-Sb-SnO2-Ti-1 electrode.

[0038] Example 2

[0039] The electrode preparation method in Example 2 was the same as in Example 1, except that in step 6), the 0.1M nickel acetate solution was replaced with a 0.1M nickel nitrate solution; all other conditions were the same as in Example 1. The electrode finally prepared in Example 2 was labeled as immersion-Ni-Sb-SnO2-Ti-2.

[0040] Example 3

[0041] The electrode preparation method in Example 3 was the same as in Example 1, except that in step 6), the 0.1M nickel acetate solution was replaced with a 0.1M nickel chloride hexahydrate solution; all other conditions were the same as in Example 1. The electrode finally prepared in Example 3 was labeled as immersion-Ni-Sb-SnO2-Ti-3.

[0042] Example 4

[0043] The electrode preparation method in Example 4 was the same as in Example 1, except that in step 6), the 0.1M nickel acetate solution was replaced with a 0.1M nickel hypophosphate solution; all other conditions were the same as in Example 1. The electrode finally prepared in Example 4 was labeled as immersion-Ni-Sb-SnO2-Ti-4.

[0044] Example 5

[0045] The electrode preparation method in Example 5 was the same as in Example 1, except that in step 6), the 0.1M nickel acetate solution was replaced with a 0.1M nickel acetylacetone solution; all other conditions were the same as in Example 1. The electrode finally prepared in Example 5 was labeled as immersion-Ni-Sb-SnO2-Ti-5.

[0046] Comparative Example 1

[0047] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0048] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0049] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride, 78 mg of antimony trichloride, and 99.54 mg of nickel acetate to the deposition solution and stir to dissolve.

[0050] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0051] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition reaction was carried out for 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140℃.

[0052] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Ni-Sb-SnO2-Ti-1.

[0053] Comparative Example 2

[0054] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0055] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0056] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride, 78 mg of antimony trichloride, and 74.4 mg of nickel nitrate to the deposition solution and stir to dissolve.

[0057] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0058] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition time was 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140°C.

[0059] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Ni-Sb-SnO2-Ti-2.

[0060] Comparative Example 3

[0061] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0062] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0063] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride, 78 mg of antimony trichloride, and 96.8 mg of nickel chloride hexahydrate to the deposition solution and stir to dissolve.

[0064] 3) Place the treated titanium sheet with a size of 2*2cm in the middle of the solution as the cathode, and place two graphite plates parallel to the cathode as the anode. The size of the graphite plates is 3*3cm. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed in the line of sight when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0065] 4) Connect the anode and cathode to the positive and negative terminals respectively, and set the current density to 10 mA / cm². 2 The electrodeposition time was 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140°C.

[0066] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Ni-Sb-SnO2-Ti-3.

[0067] Comparative Example 4

[0068] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0069] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0070] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride, 78 mg of antimony trichloride, and 132.8 mg of nickel hypophosphite to the deposition solution and stir to dissolve.

[0071] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0072] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition reaction was carried out for 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140℃.

[0073] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Ni-Sb-SnO2-Ti-4.

[0074] Comparative Example 5

[0075] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0076] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0077] 2) Prepare the electrodeposition solution by mixing choline chloride and ethylene glycol in a 1:2 molar ratio and heating at 80°C to form a colorless and transparent deposition solution. Then, measure 40 mL of the deposition solution and add 2275.2 mg of stannous chloride, 78 mg of antimony trichloride, and 104.6 mg of nickel acetylacetonate to the deposition solution and stir to dissolve.

[0078] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0079] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition reaction was carried out for 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140℃.

[0080] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Ni-Sb-SnO2-Ti-5.

[0081] Comparative Example 6

[0082] A drop-cast β-PbO2 electrode includes the following steps:

[0083] 1) First, weigh 8 mg of β-PbO2 catalyst and dissolve it in 900 μL of ethanol and 100 μL of Nafion solution. Sonicate at 700 W for 0.5 h.

[0084] 2) The mixture obtained in step 1) is applied to the surface of a titanium felt measuring 2cm*2cm and dried with an infrared lamp to obtain the electrode β-PbO2-Ti.

[0085] Comparative Example 7

[0086] A tin-antimony-nickel size-stabilized electrode prepared by electroplating and impregnation includes the following steps:

[0087] 1) First, polish the titanium sheet with 800-grit and 3000-grit sandpaper respectively. Then, immerse it in a 20wt% sodium hydroxide solution and heat it at 80°C to remove the oil. Next, immerse it in a 10% oxalic acid solution and heat it at 95°C to etch it. Finally, take out the titanium sheet and wash it with clean water.

[0088] 2) Prepare the electrodeposition solution by measuring 40 mL of deionized water, adding 2275.2 mg of stannous chloride and 78 mg of antimony trichloride to the water, and stirring to dissolve.

[0089] 3) Insert a 2*2cm processed titanium sheet into the middle of the electrodeposition solution as the cathode. Place two graphite plates parallel to the cathode as the anodes and insert them into the electrodeposition solution. The graphite plates are 3*3cm in size. Ensure that the graphite plates and titanium sheets are parallel and that the titanium sheets are not exposed when viewed at eye level, so that the graphite plates completely cover the titanium sheets.

[0090] 4) Connect the anode and cathode to the positive and negative terminals of the power supply, respectively, and set the current density to 10 mA / cm². 2 The electrodeposition reaction was carried out for 20 minutes. After obtaining the deposited titanium sheet, it was dried in an oven at 140℃.

[0091] 5) The dried titanium sheet was calcined in a muffle furnace at 600℃ for 2 hours to obtain a size-stable electrode deposit -Sb-SnO2-Ti.

[0092] 6) The obtained precipitated Sb-SnO2-Ti electrode was immersed in 50 mL of 0.1 M nickel acetate solution for 8 h, dried, and calcined in a muffle furnace at 500 °C for 2 h to obtain the precipitated Ni-Sb-SnO2-Ti-6 electrode.

[0093] Application Example 1:

[0094] The electrocatalytic ozone production performance of the catalysts in Examples 1-5 was verified respectively:

[0095] A galvanometer was used as the electrochemical generator, employing a two-electrode system with a current set to 1A. The size-stabilized electrode from Examples 1-5 was used as the anode, a platinum sheet as the counter electrode, and 0.5M sulfuric acid solution as the electrolyte. The generated ozone gas was detected using a 2B tech instrument. During the testing process, the effects of each catalyst on the gaseous ozone concentration during the electrocatalytic reaction were as follows: Figure 1 The Faraday efficiency of gaseous ozone is as follows: Figure 2 As shown.

[0096] from Figure 1-2As can be seen, the electrocatalytic activity of the size-stabilized electrodes in Examples 4 and 5 is poor. The main reason is that the different nickel sources during electrode preparation have a significant impact on their performance. Nickel hypophosphite may produce phosphides during thermal decomposition, which poison the catalyst. Nickel acetylacetonate has too high a carbon content and is only slightly soluble in water, so its adhesion during impregnation is relatively poor, and the amount of nickel oxide produced after oxidation is relatively small.

[0097] Application Example 2

[0098] The electrocatalytic ozone performance of the catalysts in Comparative Examples 1-4 was verified respectively:

[0099] An electrochemical generator was used as the electrochemical generating device, employing a two-electrode system with a current set to 1A. The stabilized electrodes of Comparative Examples 1-7 were used as the anode, a platinum sheet as the counter electrode, and 0.5M sulfuric acid solution as the electrolyte. The generated ozone gas was detected using a 2B tech instrument. During the test, the effects of each catalyst on ozone production were observed when the electrocatalytic reaction was performed using the catalysts of Comparative Examples 1-4, as shown below. Figure 3 As shown.

[0100] from Figure 3 It can be seen that the electrocatalytic activity of Comparative Examples 1-5 and 7 is relatively poor, indicating that the Ni loading step and solvent selection during electrode preparation have a significant impact on their performance. The performance of ozone is mainly compared based on current efficiency (Faraday efficiency), and the current efficiency (Faraday efficiency) of the β-PbO2 electrode in Comparative Example 6 is approximately 12%.

[0101] Application Example 3 (Testing Catalyst Lifespan):

[0102] Ozone lifetime testing

[0103] Catalysts were prepared using the size-stabilized electrodes of Example 1 and Comparative Example 1 as catalysts.

[0104] Lifetime test (current i - time t): A galvanometer was used as the electrochemical generating device. The size-stabilized electrodes of Example 1 (impregnated Ni-Sb-SnO2-Ti-1) and Comparative Example 1 (precipitated Ni-Sb-SnO2-Ti-1) were used as working electrodes, and a platinum sheet was used as the counter electrode. A 0.5M sulfuric acid aqueous solution was used as the electrolyte. During the test, the current was set to 0.5A, and the change in voltage U with time t was monitored using an electrochemical workstation. An increase in current U reflects instability and easy deactivation during a long reaction time t. The lifetime test (voltage U - time t) results in the electrocatalytic ozone production application are as follows: Figure 4 As shown.

[0105] from Figure 4It can be seen that the material prepared in Example 1 has good stability (its voltage rise was slow within 50 hours of life test, and it was deactivated after 200 hours), and has promising applications in industry.

[0106] The contents described in this specification are merely an enumeration of the implementation forms of the inventive concept, and the scope of protection of this invention should not be regarded as limited to the specific forms described in the embodiments.

Claims

1. A method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation, characterized in that... Includes the following steps: 1) The titanium sheet is polished to remove the oxide layer on its surface and roughen the surface. Then it is washed and dried to obtain a pretreated titanium sheet. 2) Then, an electrodeposition solution containing stannous salt and trivalent antimony salt is prepared. The pretreated titanium sheet is used as the cathode. The anode and cathode are inserted into the electrodeposition solution and connected to the positive and negative terminals of the power supply, respectively. Sn and Sb are electrodeposited on the titanium sheet through an electrolytic reaction. After that, the titanium sheet with Sn and Sb electrodeposited is taken out, dried, and placed in a muffle furnace for a single calcination treatment in air environment to oxidize Sn and Sb to SnO2 and Sb2O3, respectively, to obtain a precipitated-Sb-SnO2 electrode. 3) Subsequently, the immersion-Sb-SnO2 electrode was immersed in a nickel salt solution for impregnation treatment. After that, the electrode was taken out and dried, and then placed in a muffle furnace for a second calcination treatment in air environment to oxidize the nickel on the electrode to the oxidized state, thus obtaining the immersion-Ni-Sb-SnO2-Ti electrode, which is the preparation completed. In step 2), the solvent for the electrodeposition solution is prepared by mixing choline chloride and ethylene glycol, heating and dissolving them into a colorless and transparent solution, wherein the molar ratio of choline chloride to ethylene glycol is 1:1 to 1:

5. In step 2), the concentration of stannous salt in the electrodeposition solution is 0.1-1 M, and the concentration of trivalent antimony salt is 0.005-0.1 M. In step 2), when installing the cathode and anode, the titanium sheet is inserted into the middle of the solution as the cathode, and two graphite plates are placed parallel to the cathode as the anode. When viewed at eye level, the titanium sheet is not exposed, so that the graphite plates completely cover the titanium sheet. The current density during electrolysis is 5-20 mA / cm². 2 The electrodeposition time is 5-40 min; In step 3), the nickel salt is nickel acetate.

2. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... The washing in step 1) involves sequential alkaline washing to remove oil and acid washing to etch. The alkaline washing solution is NaOH solution with a concentration of 10-40 wt%, the alkaline washing temperature is 60-100 ℃, and the alkaline washing time is 0.5 h-3 h. The acid washing solution is oxalic acid solution with a mass concentration of 5%-20%, the acid washing etching time is 0.5-4 h, and the acid washing temperature is 60-100 ℃.

3. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 2, characterized in that... The NaOH solution has a concentration of 20 wt%, an alkaline washing temperature of 75-80 ℃, and an alkaline washing time of 1 h; the oxalic acid solution has a mass concentration of 10%, an acid etching time of 2 h, and an acid etching temperature of 90-95 ℃.

4. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... In step 2), after mixing choline chloride and ethylene glycol, the mixture is heated to dissolve at a temperature of 60-90 °C, and the molar ratio of choline chloride to ethylene glycol is 1:2-3.

5. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... In step 2), the concentration of stannous salt in the electrodeposition solution is 0.2-0.3 M, and the concentration of trivalent antimony salt is 0.008-0.01 M.

6. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... In step 2), the current density during electrolysis is 10 mA / cm². 2 The electrodeposition time was 20 min.

7. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... Step 2) The calcination temperature in the muffle furnace is 450 ℃-700 ℃, and the calcination time is 1-4 h.

8. The method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 7, characterized in that... Step 2) The calcination temperature in the muffle furnace is 600 ℃ and the calcination time is 2 h.

9. A method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 1, characterized in that... In step 3), the nickel salt concentration is 0.05-0.5 M, and the impregnation time is 2-12 h; in step 3), the calcination temperature in the muffle furnace is 450-700 ℃, and the calcination time is 1-4 h.

10. A method for preparing a tin-antimony-nickel size-stabilized electrode based on electroplating and impregnation as described in claim 9, characterized in that... In step 3), the nickel salt concentration is 0.1 M and the impregnation time is 6-8 h; in step 3), the calcination temperature in the muffle furnace is 500℃ and the calcination time is 2 h.

11. A size-stable electrode prepared by the method according to any one of claims 1 to 10.

12. The application of the size-stabilized electrode as described in claim 11 in the electrocatalytic preparation of ozone.

13. The application as described in claim 12, characterized in that... An electrochemical generator was used as a galvanometer, employing a two-electrode system. A Ni-Sb-SnO2-Ti size-stabilized electrode was used as the anode, a platinum sheet as the counter electrode, and sulfuric acid solution as the electrolyte to carry out an electrochemical oxidation reaction and produce ozone gas. The concentration of the sulfuric acid solution was 0.05-1 M.

14. The application as described in claim 13, characterized in that... The concentration of the sulfuric acid solution is 0.5 M.

Citation Information

Patent Citations

  • Fabrication method of long-life titanium base electrode

    CN103014755A

  • Preparation of titanium-based titanium dioxide nanometer tube decomposition tin antimony fluorine electrode and application of titanium-based titanium dioxide nanometer tube decomposition tin antimony fluorine electrode to degradation on chromium fog inhibitor in electric plating chromium waste water

    CN108328703A