A pre-lithiated silicon-based composite material, a preparation method thereof, a negative electrode and a lithium-containing battery

By using a core-shell structured pre-lithiated silicon-based composite material, uniform lithium introduction and coating were achieved, solving the problems of volume expansion and SEI film damage in lithium-ion battery anode materials during charge and discharge, and improving the battery's initial coulombic efficiency and cycle stability.

CN117747763BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211125086.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2026-11-20
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

Existing powder pre-lithiation technology is difficult to achieve stable introduction of high lithium content, which leads to volume expansion, SEI film damage and reduced coulombic efficiency of lithium-ion battery anode materials during charge and discharge, affecting battery cycle performance and lifespan.

Method used

The pre-lithiated silicon-based composite material with a core-shell structure has a porous silicon matrix and a lithium-containing core component in the core, and is coated with a first carbon layer and a second carbon layer in sequence on the outside. The uniform introduction and coating of lithium is achieved through solid-phase homogenization, spray granulation and sintering treatment, avoiding the increase of slurry pH.

Benefits of technology

It significantly improves the initial coulombic efficiency and cycle stability of lithium-ion batteries, suppresses slurry gas generation, and enhances the capacity cycle stability of batteries and the stability of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117747763B_ABST
    Figure CN117747763B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a pre-lithiated silicon-based composite material, a preparation method thereof, a negative electrode and a lithium-containing battery. The pre-lithiated silicon-based composite material comprises pre-lithiated silicon-based composite particles with a core-shell structure, the inner core of the pre-lithiated silicon-based composite particles comprises a porous silicon matrix and an inner core lithium-containing component dispersed on the surface and in the pores of the silicon matrix; the outer surface of the inner core is sequentially coated with a first carbon layer and a second carbon layer from inside to outside, and the first carbon layer and the second carbon layer form an outer shell with a core-shell structure. The present disclosure introduces lithium elements into the silicon-based inner core, achieves the purpose of pre-introducing high lithium content, and can also improve the cycle performance and stability of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to lithium-ion battery materials, specifically to a pre-lithiated silicon-based composite material and its preparation method, a negative electrode, and a lithium-containing battery. Background Technology

[0002] Among novel anode materials, silicon has attracted much attention due to its high theoretical capacity, abundant reserves, and low discharge voltage. However, silicon exhibits significant volume expansion (>300%) during lithium insertion / extraction, leading to pulverization and detachment of the anode material, forming "dead silicon," and ultimately causing the anode material to lose electrical contact, resulting in battery failure. Furthermore, repeated volume expansion and contraction also cause the surface SEI film to continuously break down and form, constantly consuming the Li₂ of the cathode. + This leads to a decrease in battery coulombic efficiency. These problems ultimately cause a sharp deterioration in battery cycle performance, severely impacting battery lifespan.

[0003] Pre-lithiation technology provides an effective solution to address irreversible capacity loss and improve coulombic efficiency. Powder pre-lithiation is one of the most direct and effective means to improve the initial coulombic efficiency of silicon anodes. By introducing exogenous lithium into the battery system in a suitable manner and form, the reduction in initial coulombic efficiency caused by the consumption of effective lithium by the silicon anode can be mitigated. However, it is currently difficult to increase the lithium content in powder pre-lithiation. When the lithium content is high, the lithium on the material surface makes the material unstable and difficult to store. Furthermore, during application, it easily causes the pH of the slurry to rise during the slurry preparation process, reacting with binders and / or solvent water, resulting in gas generation and difficulty in slurry preparation, which in turn degrades battery performance.

[0004] Currently, the structure and carbon coating process conditions for pre-lithiated powder cannot produce pre-lithiated powder materials with ideal properties (such as high stability); nor can they effectively avoid the phenomenon of increased slurry pH caused by the application of lithium-added powder during slurry preparation. Summary of the Invention

[0005] The purpose of this disclosure is to provide a pre-lithiated silicon-based composite material and its preparation method, a negative electrode and a lithium-containing battery, which can achieve the purpose of high lithium content pre-introduction, improve the coating density of the carbon layer on the surface of the pre-lithiated silicon-based composite material, and improve the first coulombic efficiency and cycle stability of the lithium-containing battery when the composite material is used.

[0006] To achieve the above objectives, the first aspect of this disclosure provides a pre-lithiated silicon-based composite material comprising core-shell structured pre-lithiated silicon-based composite particles. The core of the pre-lithiated silicon-based composite particles comprises a porous silicon matrix and a core lithium-containing component dispersed on the surface and within the pores of the silicon matrix. The outer surface of the core is sequentially coated with a first carbon layer and a second carbon layer from the inside out, and the first carbon layer and the second carbon layer form a core-shell structured outer shell.

[0007] Optionally, the first carbon layer contains a first lithium-containing component, and the second carbon layer is lithium-free; wherein the lithium content in the core is greater than the lithium content in the first carbon layer; optionally, the lithium-containing component in the core contains one or more of lithium silicon alloy, lithium silicate, and lithium oxide; the first lithium-containing component contains one or more of lithium carbide, lithium silicate, and lithium oxide.

[0008] Optionally, the total thickness of the first carbon layer and the second carbon layer is 10–1000 nm; optionally, the thickness of the first carbon layer is 10–500 nm, and the thickness of the second carbon layer is 5–500 nm; optionally, the average particle size of the pre-lithiated silicon-based composite particles is 0.5–30 μm, the average pore size is 1–30 nm, and the BET specific surface area is 0.5–50 m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g.

[0009] The second aspect of this disclosure provides a method for preparing a pre-lithiated silicon-based composite material, the method comprising the following steps: S1, mixing metallic lithium with porous silicon-based material powder, and then performing solid-phase homogenization treatment to obtain a first mixture; S2, adding a solid dispersant to the first mixture for dispersion homogenization treatment to obtain a second mixture; S3, mixing and homogenizing a carbonizable organic carbon source binder, a solvent, and the second mixture to obtain a mixed slurry; S4, performing spray granulation treatment on the mixed slurry to obtain a pre-lithiated composite material precursor; S5, performing sintering treatment on the pre-lithiated composite material precursor; the above steps S1 to S5 are carried out in an inert atmosphere.

[0010] Optionally, in step S1, the porous silicon-based material powder has an average particle size of 0.5–10 μm, an average pore size of 0.5–30 nm, and a BET specific surface area of ​​0.1–100 m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g; the lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powder or lithium sheets; optionally, the weight ratio of the lithium metal to the porous silicon-based material powder is 1:(1-100), preferably 1:(5-50).

[0011] Optionally, before step S1, the method further includes: acid etching the silicon alloy raw material with acid, followed by washing and drying to obtain the porous silicon-based material powder; optionally, the silicon alloy is selected from one or more of silicon-aluminum alloy, silicon-iron alloy, and silicon-magnesium alloy; the silicon content in the silicon alloy raw material is 30-70% by weight.

[0012] Optionally, in step S1, the solid phase homogenization treatment method includes mechanical homogenization, wherein the mechanical homogenization is selected from any one of ball mill, sand mill, homogenizer or disperser; Optionally, in step S1, the rotation speed of the solid phase homogenization treatment is 300 to 2000 r / min, the homogenization time is 6 to 72 h, and the ball-to-material ratio is (1 to 30): 1.

[0013] Optionally, in step S2, the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon and soft carbon; the weight ratio of the solid dispersant to the lithium metal is (1-50):1, preferably (5-10):1.

[0014] Optionally, in step S2, the dispersion and homogenization process includes mechanical homogenization, which is selected from any one of ball mill, sand mill, homogenizer or disperser; the rotation speed of the dispersion and homogenization process is 50 to 500 r / min, the time is 0.5 to 12 h, and the ball-to-material ratio is (1 to 50): 1.

[0015] Optionally, in step S3, the organic carbon source binder is selected from one or more of polymer carbon sources, petroleum carbon sources, sugar carbon sources, graphite carbon sources, and other carbon sources; the polymer carbon source includes one or more of phenolic resin, epoxy resin, polyvinylpyrrolidone, and polyvinyl alcohol; the petroleum carbon source includes one or more of asphalt, petroleum coke, and needle coke; the sugar carbon source includes one or more of glucose, sucrose, and fructose; the other carbon source is selected from one or more of sodium carboxymethyl cellulose, polyvinyl alcohol, and carboxylated styrene-butadiene latex; the solvent is selected from one or more of ethanol, isopropanol, n-butanol, cyclohexane, and cyclohexanone; preferably, the weight ratio of the organic carbon source binder to lithium metal is (10-100):1, more preferably (40-80):1; the weight ratio of the solvent to the organic carbon source binder is (10-50):1.

[0016] Optionally, in step S4, the conditions for spray granulation include: an inlet temperature of 100–300°C, an outlet temperature of 50–200°C, a carrier gas flow rate of 10–100 L / min, and a pressure of -0.1 to -0.08 MPa; preferably, the inlet temperature is 120–240°C, the outlet temperature is 80–150°C, the carrier gas flow rate is 30–60 L / min, and the pressure is -0.1 to -0.05 MPa.

[0017] Optionally, in step S5, the sintering process includes a first-stage sintering and a second-stage sintering; wherein the temperature of the first-stage sintering is 200–500°C, the heating rate is 1–3°C / min, and the holding time is 1–6 h; the temperature of the second-stage sintering is 500–1200°C, the heating rate is 1–5°C / min, and the holding time is 1–12 h; preferably, the temperature of the first-stage sintering is 250–400°C, the heating rate is 2–3°C / min, and the holding time is 2–3 h; the temperature of the second-stage sintering is 700–900°C, the heating rate is 2–3°C / min, and the holding time is 2–6 h.

[0018] Optionally, the inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton, and xenon; the water content of the inert atmosphere is less than 0.1% by weight, and the oxygen content is less than 0.1% by weight.

[0019] A third aspect of this disclosure provides a pre-lithiated silicon-based composite material prepared according to the method described in the second aspect of this disclosure.

[0020] This disclosure provides a fourth aspect of a lithium-ion battery negative electrode comprising the pre-lithiated silicon-based composite material described in the first or third aspect of this disclosure.

[0021] This disclosure provides a lithium-ion battery, including the negative electrode described in the fourth aspect of this disclosure.

[0022] Through the above technical solution, this disclosure provides a pre-lithiated silicon-based composite material and its preparation method, a negative electrode, and a lithium-containing battery. The pre-lithiated silicon-based composite material comprises pre-lithiated silicon-based composite particles, realizing the pre-introduction of lithium elements into the surface and channels of the porous silicon matrix core. Furthermore, a first carbon layer and a second carbon layer are sequentially coated on the outside of the core. The first carbon layer ensures the uniformity of the lithium-containing silicon-based material coating, preventing direct contact between the core and the external environment, further improving the material's cycle performance and stability. The second carbon coating layer is lithium-free, preventing pH increase in the slurry during homogenization and suppressing gas generation. When applied to lithium-ion battery negative electrode materials, the pre-lithiated silicon-based composite material significantly improves the battery's initial coulombic efficiency and cycle stability. Moreover, the high lithium content in the composite material core continuously releases and replenishes lithium during charge-discharge cycles, compensating for lithium-ion consumption and loss during battery cycling, and improving capacity cycle stability (e.g., improving post-cycle capacity retention).

[0023] Furthermore, the method for preparing pre-lithiated silicon-based composite materials disclosed herein first introduces lithium through a solid-state homogenization reaction, forming a silicon-lithium alloy and / or lithium oxide on the surface and within the pores of the silicon matrix. Then, a first carbon layer is formed through a dispersion homogenization process, followed by spray drying and subsequent sintering to form a second carbon layer. Spray granulation facilitates the formation of a uniform and dense carbon coating layer. Sintering allows most of the lithium to diffuse into the pores of the silicon matrix, achieving pre-lithiation, while limiting the temperature range to inhibit the growth of silicon grains within the silicon particles, thereby improving the initial coulombic efficiency and cycle stability of the silicon-based anode material. However, a small amount of lithium diffuses into the first carbon layer, forming a carbon-lithium alloy and / or lithium oxide. This method is compatible with existing lithium-ion battery anode material systems and can be directly applied to them. Simultaneously, this method features controllable lithium content, simple process, easy operation, environmental friendliness, low cost, and ease of scalability.

[0024] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0025] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings:

[0026] Figure 1 This is a schematic diagram of the structure of the pre-replenished lithium-silicon-based composite material provided in this disclosure;

[0027] Figure 2 Here is a scanning electron microscope image of the product obtained in Example 1 of this disclosure;

[0028] Figure 3 The X-ray diffraction pattern of the product obtained in Example 1 of this disclosure;

[0029] Figure 4 The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of the product obtained in Example 1 of this disclosure;

[0030] Figure 5 The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of the intermediate product obtained in Example 1;

[0031] Figure 6 The first charge-discharge curve of a lithium-ion battery using the product obtained in Example 1 of this disclosure as the negative electrode material at a current density of 0.2C is shown.

[0032] Figure 7The cycling performance of a lithium-ion battery using the product obtained in Example 1 of this disclosure as the negative electrode material is evaluated at a current density of 0.2C and at current densities of 0.5C, 1.0C, and 5.0C.

[0033] Figure 8 The capacity retention rate of lithium-ion batteries using the product obtained in Example 1 of this disclosure as the negative electrode material at current densities of 0.2C, 0.5C, 1.0C, and 5.0C.

[0034] Figure 9 This is a transmission electron microscope image of the product obtained in Example 1 of this disclosure. Detailed Implementation

[0035] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.

[0036] The first aspect of this disclosure provides a pre-lithiated silicon-based composite material, such as... Figure 1 As shown, the pre-lithiated silicon-based composite material comprises pre-lithiated silicon-based composite particles with a core-shell structure. The core of the pre-lithiated silicon-based composite particles comprises a porous silicon matrix and a core lithium-containing component dispersed on the surface and in the pores of the silicon matrix. The outer surface of the core is covered with a first carbon layer and a second carbon layer from the inside out, and the first carbon layer and the second carbon layer form a core-shell structure.

[0037] This disclosure provides a pre-lithiated silicon-based composite material that pre-introduces lithium into the surface and pores of a porous silicon matrix core. A first carbon layer and a second carbon layer are sequentially coated around the core. The first carbon layer ensures uniform coating of the lithium-containing silicon-based material, preventing direct contact between the core and the external environment, thus further improving the material's cycle performance and stability. The second carbon coating layer is lithium-free, preventing pH increases in the slurry during homogenization and suppressing gas generation. When applied to lithium-ion battery anode materials, this pre-lithiated silicon-based composite material significantly improves the battery's initial coulombic efficiency and cycle stability. Furthermore, the high lithium content in the composite core continuously releases and replenishes lithium during charge-discharge cycles, compensating for lithium-ion consumption and loss during battery cycling, and improving capacity cycle stability.

[0038] According to this disclosure, the general chemical formula of the silicon-lithium alloy is SiLi. x , where 0 < x ≤ 10.

[0039] In one embodiment, the total thickness of the first carbon layer and the second carbon layer is 10-1000 nm; the thickness of the first carbon layer is 10-500 nm, and the thickness of the second carbon layer is 5-500 nm.

[0040] In a preferred embodiment, the total thickness of the first carbon layer and the second carbon layer is 50-500 nm; the thickness of the first carbon layer is 10-100 nm, and the thickness of the second carbon layer is 5-100 nm.

[0041] In this disclosure, the thicknesses of the first and second carbon layers were obtained by transmission electron microscopy (TEM) measurements.

[0042] In a preferred embodiment, in the pre-lithiated silicon-based composite particles, the first carbon layer contains a first lithium-containing component, and the second carbon layer is lithium-free; preferably, the lithium content in the core is greater than the lithium content in the first carbon layer.

[0043] In one specific embodiment, the core lithium-containing component comprises one or more of lithium metal, lithium silicon alloy, and lithium oxide; the first lithium-containing component comprises one or more of lithium carbide, lithium silicate, and lithium oxide.

[0044] According to the general chemical formula of the lithium-carbon alloy disclosed herein, Li y C, where 0 <y≤6。

[0045] The pre-lithiated silicon-based composite material disclosed herein consists of a core, a first carbon layer, and a second carbon layer, with the lithium content decreasing in that order, exhibiting a gradient distribution. The core has the highest lithium content, which is beneficial for improving capacity cycling stability. The second carbon layer is lithium-free, which can further prevent the pH of the slurry from increasing during homogenization and suppress gas generation in the slurry.

[0046] In one embodiment, the pre-lithiated silicon-based composite particles have an average particle size of 0.5–30 μm, an average pore size of 1–30 nm, and a BET specific surface area of ​​0.5–50 m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g; preferably, the pre-lithiated silicon-based composite particles have an average particle size of 1–10 μm, an average pore size of 5–26 nm, and a BET specific surface area of ​​0.5–20 m² / g. 2 / g, total pore volume is 0.005~0.1cm³ 3 / g.

[0047] A second aspect of this disclosure provides a method for preparing a pre-lithiated silicon-based composite material, the method comprising the following steps:

[0048] S1. Mix lithium metal with porous silicon-based material powder, and then perform solid-phase homogenization treatment to obtain the first mixture.

[0049] S2. Add the solid dispersant to the first mixture and perform dispersion and homogenization treatment to obtain the second mixture;

[0050] S3. The carbonizable organic carbon source binder, solvent and the second mixture are mixed and homogenized to obtain a mixed slurry;

[0051] S4. The mixed slurry is subjected to spray granulation treatment to obtain a pre-lithiated composite material precursor;

[0052] S5. The pre-lithiated composite material precursor is subjected to sintering treatment;

[0053] The above steps S1 to S5 are carried out in an inert atmosphere.

[0054] The method for preparing pre-lithiated silicon-based composite materials disclosed herein first introduces lithium through a solid-state homogenization reaction, forming a lithium silicon alloy, lithium silicate, and lithium oxide on the surface and within the pores of a silicon matrix. Then, a first carbon layer is formed through a dispersion homogenization process, followed by spray drying and subsequent sintering to form a second carbon layer. The sintering process allows most of the lithium to diffuse into the pores of the silicon matrix, achieving pre-lithiation. Simultaneously, a limited temperature range inhibits the growth of silicon grains within the silicon particles, thereby improving the initial coulombic efficiency and cycle stability of the silicon-based anode material. However, a small amount of lithium diffuses into the first carbon layer, forming lithium carbide, lithium silicate, and lithium oxide. This method is compatible with existing lithium-ion battery anode material systems and can be directly applied to them. Furthermore, this method features controllable lithium content, simple process, easy operation, environmental friendliness, low cost, and ease of scalability.

[0055] According to this disclosure, the inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton, and xenon; the water content of the inert atmosphere is less than 0.1% by weight, and the oxygen content is less than 0.1% by weight.

[0056] In one embodiment, the porous silicon-based material powder has an average particle size of 0.5–10 μm, an average pore size of 0.5–30 nm, and a BET specific surface area of ​​0.1–100 m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g;

[0057] The lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powder, or lithium sheets.

[0058] In one embodiment, the weight ratio of the lithium metal to the porous silicon-based material powder is 1:(1-100), preferably 1:(5-50).

[0059] The porous silicon-based material powder described in this disclosure can be purchased through conventional channels or prepared using methods known in the art.

[0060] In one specific embodiment, before step S1, the method further includes:

[0061] The silicon alloy raw material is subjected to acid etching treatment, followed by washing and drying to obtain the porous silicon-based material powder.

[0062] Optionally, the silicon alloy is selected from one or more of silicon-aluminum alloy, silicon-iron alloy, and silicon-magnesium alloy; the silicon content in the silicon alloy raw material is 30-70% by weight. The acid used for acid etching is selected from one or more of hydrochloric acid, sulfuric acid, oxalic acid, phosphoric acid, methanesulfonic acid, aminosulfonic acid, and citric acid. The specific process conditions for acid etching in this disclosure are conventional operating conditions in the art.

[0063] This disclosure employs acid etching of a silicon alloy to obtain the porous silicon raw material. The porous silicon bulk obtained through silicon alloy etching is easier to pulverize than ordinary silicon bulk, facilitating the preparation of nano-silicon materials. Furthermore, the reduced pulverization time also minimizes oxidation during the grinding process. Moreover, by modifying inexpensive silicon alloy materials to introduce a porous structure within the material, the low cost and ease of large-scale production promote the practical application of silicon-based anode materials.

[0064] In one embodiment, in step S1, the solid phase homogenization process includes mechanical homogenization, wherein the mechanical homogenization is selected from any one of a ball mill, a sand mill, a homogenizer, or a disperser.

[0065] Optionally, in step S1, the rotation speed of the solid phase homogenization treatment is 300-2000 r / min, the homogenization time is 6-72 h, and the ball-to-material ratio is (1-20):1.

[0066] In one embodiment, in step S2, the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, and soft carbon.

[0067] The weight ratio of the solid dispersant to the lithium metal is (1-50):1, preferably (5-10):1.

[0068] This disclosure uses a solid dispersant to prevent silicon and lithium from agglomerating during the ball milling reaction, thus ensuring that the silicon-lithium particles are fully dispersed. At the same time, the dispersant can also form a diffusely distributed conductive network, increasing the conductivity of the particles and suppressing the decrease in conductivity caused by the introduction of lithium.

[0069] In one embodiment, in step S2, the dispersion and homogenization process includes mechanical homogenization, wherein the mechanical homogenization is selected from any one of a ball mill, a sand mill, a homogenizer, or a disperser.

[0070] The dispersion and homogenization treatment is carried out at a rotation speed of 50-500 r / min for 0.5-12 h, with a ball-to-material ratio of (1-50):1.

[0071] In one embodiment, in step S3, the organic carbon source binder is selected from one or more of polymer carbon sources, petroleum-based carbon sources, sugar-based carbon sources, graphite-based carbon sources, and other carbon sources;

[0072] The polymer carbon source includes one or more of phenolic resin, epoxy resin, polyvinylpyrrolidone, and polyvinyl alcohol;

[0073] The petroleum-based carbon sources include one or more of pitch, petroleum coke and needle coke;

[0074] The carbohydrate carbon source includes one or more of glucose, sucrose, and fructose;

[0075] The other carbon source is selected from one or more of sodium carboxymethyl cellulose, polyvinyl alcohol, and carboxylated styrene-butadiene latex; preferably, it is selected from one or more of sodium carboxymethyl cellulose.

[0076] The solvent is selected from one or more of ethanol, isopropanol, n-butanol, cyclohexane, and cyclohexanone;

[0077] Preferably, the weight ratio of the organic carbon source binder to lithium metal is 10 to 100:1, more preferably 40 to 80:1;

[0078] The weight ratio of the solvent to the organic carbon source binder is 10 to 50:1.

[0079] In one embodiment, in step S4, the conditions for spray granulation include: an inlet temperature of 100–300°C, an outlet temperature of 50–200°C, a carrier gas flow rate of 30–60 L / min, and a pressure of -0.1–-0.05 MPa. This disclosure uses a mixed slurry for spray granulation, which is beneficial for improving the uniformity of the second carbon layer coating and avoids damage to the particle pore structure.

[0080] In a preferred embodiment, in step S4, the conditions for spray granulation include: an inlet temperature of 120–240°C, an outlet temperature of 80–150°C, a carrier gas flow rate of 30–60 L / min, and a pressure of -0.1–-0.05 MPa. The composite material prepared according to this embodiment has a denser second carbon layer and produces less gas in the slurry, further improving the stability of the composite material in lithium-ion battery anode materials.

[0081] In one embodiment, step S5 includes a first-stage sintering and a second-stage sintering. The temperature of the first-stage sintering is 200–500°C, the heating rate is 0.1–3°C / min, and the holding time is 1–6 h. The temperature of the second-stage sintering is 500–1200°C, the heating rate is 1–5°C / min, and the holding time is 1–12 h.

[0082] In a preferred embodiment, the sintering temperature of the first stage is 250–400°C, the heating rate is 2–3°C / min, and the holding time is 2–3 h; the sintering temperature of the second stage is 700–900°C, the heating rate is 2–3°C / min, and the holding time is 2–6 h.

[0083] The inventors of this disclosure have discovered that by performing thermal stabilization through segmented heating sintering and limiting the thermal stabilization temperature within the aforementioned range, the growth of silicon grains inside the silicon particles can be suppressed, further preventing a decrease in cycle stability.

[0084] A third aspect of this disclosure provides a pre-lithiated silicon-based composite material prepared according to the method described in the second aspect of this disclosure.

[0085] This disclosure provides a fourth aspect of a lithium-ion battery negative electrode, comprising the pre-lithiated silicon-based composite material described in the first or third aspect of this disclosure.

[0086] According to this disclosure, the negative electrode can be prepared using methods known in the art. For example, the negative electrode is obtained by slurry coating, wherein the slurry includes the pre-lithiated silicon-based composite material, conductive agent, binder, etc. provided in this disclosure, and the conductive agent and binder are conventionally selected in the art.

[0087] The fifth aspect of this disclosure provides a lithium-ion battery comprising the negative electrode described in the fourth aspect of this disclosure.

[0088] According to this disclosure, lithium-ion batteries can be assembled using methods known in the art.

[0089] The pre-lithiated silicon-based composite material disclosed herein can be directly applied to existing lithium-ion battery anode systems, and can also be used in combination with lithium-ion battery graphite anode materials, silicon-carbon anode materials, and silicon suboxide anode materials. When this pre-lithiated silicon-based composite material is applied to lithium-ion batteries, it significantly improves the initial coulombic efficiency and cycle stability of the lithium-ion battery.

[0090] The present disclosure will be further illustrated by the following examples, but the present disclosure is not limited thereto.

[0091] Unless otherwise specified, all raw materials used in the following embodiments are commercially available products.

[0092] In the following embodiments, the specific test methods are as follows:

[0093] The average particle size was tested using a particle size analyzer, specifically a Mastersizer 3000 instrument.

[0094] The average pore size, BET specific surface area, and total pore volume were measured using a specific surface area and pore size analyzer JW-BK100.

[0095] The SEM testing method was a scanning electron microscope, and the instrument model was Hitachi S4800 from Japan.

[0096] The TEM test method was transmission electron microscopy, and the instrument model was Hitachi FEI G2F20 from Japan.

[0097] The XRD test method was an X-ray diffractometer, specifically the PANalytical X'Pert PRO powder X-ray diffractometer.

[0098] The XPS test method is X-ray photoelectron spectroscopy, and the instrument model is VG ESCALAB;

[0099] The electrochemical cycling performance was tested using the Blue Electric Test System, instrument model CT3001A.

[0100] Preparation Example 1

[0101] This preparation example illustrates the preparation of porous silicon-based material powder, specifically including: using a silicon-aluminum alloy with a silicon content of 60% by weight in an excess of 1 mol L⁻¹. -1 Hydrochloric acid etching was performed for 12 hours. After the reaction was complete, the powder was washed with deionized water until neutral and then dried in a vacuum oven at 60°C for 12 hours to obtain porous silicon powder, denoted as G-1.

[0102] Testing revealed that the G-1 product had an average particle size of 2.8 μm, an average pore size of 8.23 ​​nm, and a BET specific surface area of ​​2.14 m². 2 / g, total pore volume is 0.005cm³ 3 / g.

[0103] Preparation Example 2

[0104] This preparation example illustrates the preparation of porous silicon-based material powder, specifically including: using a silicon-aluminum alloy with a silicon content of 70% by weight in an excess of 1 mol L⁻¹. -1 Sulfuric acid etching was performed for 20 hours. After the reaction was complete, the powder was washed with deionized water until neutral and dried in a vacuum oven at 60°C for 12 hours to obtain porous silicon powder, denoted as G-2.

[0105] Testing revealed that the G-2 product had an average particle size of 3.7 μm, an average pore size of 7.815 nm, and a BET specific surface area of ​​1.56 m². 2 / g, total pore volume is 0.013cm³ 3 / g.

[0106] Example 1

[0107] In an inert atmosphere, 2 g of porous silica powder G-1 and 0.02 g of lithium metal ingot were weighed and placed in a zirconia ball mill jar (lithium metal to porous silica weight ratio of 1:100). After sealing, the jar was transferred to a planetary ball mill for ball milling. The ball-to-material ratio was 20:1, and the zirconia balls had diameters of 5.5 mm, 3.0 mm, and 2.0 mm in a ratio of 2:5:3. The ball milling speed was 500 r / min, and the milling time was 12 h. Then, 0.1 g of natural graphite was added and ball milling continued (lithium metal to solid dispersant weight ratio of 1:5). The ball milling speed was 450 r / min, and the milling time was 2 h. The product obtained in this step was taken as an intermediate product.

[0108] 0.2 g of sodium carboxymethyl cellulose and 1.0 g of pitch (weight ratio of lithium metal to organic carbon source binder is 1:60) were added, along with 30 g of cyclohexane solvent (weight ratio of solvent to organic carbon source binder is 25:1). The ball milling speed was 450 r / min, and the milling time was 2 h to obtain a slurry containing lithium silicon-based composite material. The slurry was then spray-granulated under the following conditions: inlet temperature 300℃, outlet temperature 200℃, carrier gas (argon) flow rate 45 L / min, and pressure -0.05 MPa, to obtain a precursor of lithium silicon-based composite material. The precursor was then placed in a tube furnace under an argon atmosphere for thermal stabilization and sintering. The calcination process involved first heating to 500℃ at a rate of 2℃ / min for preheating and stabilization, holding at that temperature for 2 h, and then heating to 900℃ at a rate of 5℃ / min and holding at that temperature for 2 h. After cooling to room temperature, the pre-lithiated silicon composite material is obtained and denoted as A1.

[0109] The scanning electron microscope image of product A1 is shown below. Figure 2 As shown, by Figure 2 It can be seen that the pre-lithiated silicon-based composite material is granular.

[0110] Transmission electron microscopy image of product A1 is shown below Figure 9 As shown, by Figure 9 It can be seen that the pre-lithiated silicon-based composite material has a two-layer carbon-coated structure.

[0111] The X-ray diffraction pattern of product A1 is as follows: Figure 3 As shown, Figure 3 A sharp carbon peak appeared, combined with Figure 2The microstructure shown indicates that the pre-lithiated silicon-based composite material is densely coated with a carbon layer; and Figure 3 In addition to silicon peaks, the spectrum also showed obvious silicon-lithium alloy SiLi. 4.25 The characteristic peaks indicate that lithium was successfully introduced into the silicon-based material and pre-lithiation was achieved by forming a thermodynamically stable silicon-lithium alloy.

[0112] The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of product A1 is as follows: Figure 4 As shown, Figure 4 No characteristic peaks of Li were observed. Figure 5 The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of the intermediate product (lithium-silicon-based material without a second carbon coating layer) prepared in this embodiment is shown below. Figure 5 The presence of a distinctly sharp Li characteristic peak indicates that... Figure 4 and Figure 5 The comparison shows that the second carbon coating of the final product A1 obtained by using the method provided in this disclosure does not contain lithium.

[0113] Figure 6 The first charge-discharge curve of a lithium-ion battery using the product obtained in Example 1 of this disclosure as the negative electrode material is shown at a current density of 0.2C. The first charge specific capacity is 404 mAh / g, the first discharge specific capacity is 478 mAh / g, and the first coulombic efficiency is 84.5%.

[0114] Figure 7 The first charge-discharge curves of a lithium-ion battery using product A1 obtained in Example 1 of this disclosure as the negative electrode material are shown at current densities of 0.2C, 0.5C, 1.0C, and 5.0C. It can be seen that as the charge-discharge process proceeds, the specific capacity gradually increases and stabilizes at around 450mAh / g; when the current density is increased to 1.0C, the specific capacity is around 360mAh / g; when the current density drops to 0.2C after a 5.0C charge-discharge rate, the specific capacity rapidly recovers, showing good rate performance and cycle stability.

[0115] Figure 8 The cycling performance of a lithium-ion battery using product A1 obtained in Example 1 of this disclosure as the negative electrode material is shown at a current density of 0.2C and at current densities of 0.5C, 1.0C, and 5.0C. It can be seen that the capacity retention rate is still greater than 86% after 400 cycles, indicating that the pre-compensated lithium silicon-based composite material provided in this disclosure can effectively improve the cycle stability of the battery.

[0116] Comparative Example 1

[0117] The same method as in Example 1 was used, except that sodium carboxymethyl cellulose and pitch were not added during spray drying. Instead, the solid homogenized reaction product was prepared into a slurry and then spray granulated. The rest of the process and preparation conditions were the same as in Example 1. The resulting product was coated with only one layer of carbon coating and was designated as D-1.

[0118] Comparative Example 2

[0119] In an inert atmosphere, 2g of porous silicon powder G-1 was weighed and placed in a zirconia ball mill jar. After sealing, it was transferred to a planetary ball mill for ball milling. The ball-to-powder ratio was 20:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The ball milling speed was 500 r / min, and the milling time was 12 h. Then, 0.1g of natural graphite was added, and ball milling continued at a speed of 450 r / min for 2 h. The powder was then removed to obtain lithium-free porous silicon, denoted as D-2.

[0120] Example 2

[0121] In an inert atmosphere, 2g of porous silica powder G-2 and 0.04g of lithium metal ingot were weighed and placed in a zirconia ball mill jar (the weight ratio of lithium metal to porous silica was 1:50). After sealing, the jar was transferred to a planetary ball mill for ball milling. The ball-to-material ratio was 30:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The ball milling speed was 800 r / min, and the milling time was 12 h. Then, 0.4g of artificial graphite was added and ball milling continued (the weight ratio of lithium metal to solid dispersant was 1:10). The ball milling speed was 300 r / min, and the milling time was 2 h. 2g of organic carbon source binder (including 0.5g of sodium carboxymethyl cellulose and 1.5g of pitch) was added (the weight ratio of lithium metal to organic carbon source binder was 1:50), and 30g of solvent cyclohexane was added (the weight ratio of solvent to organic carbon source binder was 15:1). The ball milling speed was 300 r / min, and the ball milling time was 5h to obtain a slurry of lithium-silicon-based composite material. The above slurry was spray-granulated under the following process conditions: inlet temperature 240℃, outlet temperature 150℃, carrier gas (argon) flow rate 50L / min, and pressure -0.05MPa to obtain a precursor of lithium-silicon-based composite material. The precursor of lithium-silicon-based composite material was placed in a tube furnace under an argon atmosphere for thermal stabilization and sintering. The calcination process was as follows: first, the temperature was increased to 500℃ at a rate of 1℃ / min for preheating and stabilization, and then held at that temperature for 3h; then, the temperature was increased to 800℃ at a rate of 5℃ / min and held at that temperature for 2h. After cooling to room temperature, the pre-lithiated silicon composite material is obtained and denoted as A2.

[0122] Example 3

[0123] This embodiment refers to Example 1 for preparing the composite material, except that in the thermal stabilization sintering process, the calcination process involves first heating to 400°C at a rate of 2°C / min, holding at that temperature for 2 hours for preheating and stabilization, and then heating to 800°C at a rate of 3°C / min, holding at that temperature for 3 hours. After cooling to room temperature, the lithium-added silicon-based composite material is obtained and denoted as A3.

[0124] Example 4

[0125] This embodiment prepares the composite material according to the preparation method and process conditions of Example 1, the only difference being that the spray granulation process conditions include:

[0126] The inlet temperature was 240℃, the outlet temperature was 150℃, the carrier gas flow rate was 50L / min, and the pressure was -0.05MPa. The rest of the process was the same as in Example 1, and the resulting product was denoted as A4.

[0127] Example 5

[0128] This embodiment prepares the composite material according to the preparation method and process conditions of Example 1, with the only difference being:

[0129] A one-step sintering method is used for thermal stabilization treatment, specifically including:

[0130] The lithium-containing silicon-based composite material precursor was placed in a tube furnace under an argon atmosphere for thermal stabilization sintering. The calcination process involved heating to 900℃ at a rate of 3℃ / min and holding at that temperature for 2 hours. After cooling to room temperature, the lithium-containing silicon-based composite material, denoted as A-5, was obtained.

[0131] Example 6

[0132] This embodiment prepares the composite material according to the preparation method and process conditions of Example 1, with the only difference being:

[0133] Weigh out 2g of G-1 porous silicon and 0.1g of lithium metal ingot (lithium to porous silicon weight ratio is 1:20);

[0134] Add 0.5g of natural graphite and continue ball milling (lithium to solid dispersant weight ratio is 1:5);

[0135] A slurry was prepared by adding 1g of sodium carboxymethyl cellulose, 4g of asphalt, and 100g of organic solvent (the weight ratio of organic carbon source binder to lithium metal was 50:1, and the weight ratio of solvent to organic carbon source binder was 20:1); the remaining process was the same as in Example 1, and a pre-replenished lithium silicon-based composite material was obtained, denoted as A6.

[0136] Comparative Example 3

[0137] The negative electrode material was prepared using the method disclosed in Example 1 of CN109075330A, specifically including the following steps:

[0138] A raw material (gasification starting material) composed of mixed metallic silicon and silicon dioxide is placed in a reactor and vaporized in an environment with a vacuum of 10 Pa. The resulting substance is deposited on an adsorption plate and, after sufficient cooling, the deposit (SiO₂) is removed. x The silicon compound particles were pulverized using a jet mill (where x = 0.5). Subsequently, a carbon coating was applied to the surface of the silicon compound particles using thermal decomposition chemical vapor deposition with methane gas. Next, the carbon-coated silicon compound particles were immersed in a solution (solution A) containing lithium flakes and biphenyl dissolved in tetrahydrofuran (THF). The solution temperature was set to 20°C, and the immersion time was set to 10 hours. The silicon compound particles were then filtered out. Through the above treatment, lithium is inserted into the silicon compound particles. Subsequently, the lithium-inserted silicon compound particles were immersed in a solution (solution B) containing naphthalene dissolved in THF. The solution temperature was set to 20°C, and the immersion time was set to 20 hours. The silicon compound particles were then filtered out. Subsequently, the lithium-containing silicon compound particles were heated to a maximum temperature of 400°C in an argon environment, then cleaned, and dried under reduced pressure. This process was repeated to produce silicon-based active materials (silicon-based active material particles), and the resulting product was designated D-3.

[0139] The structural feature test data of the products obtained from the above embodiments and comparative examples are listed in Table 1 below.

[0140] Table 1

[0141]

[0142]

[0143] Test case

[0144] This test example illustrates the electrochemical performance of the products obtained in the examples and comparative examples when used as negative electrodes in lithium-ion batteries.

[0145] The products obtained in the examples and comparative examples were used as negative electrodes to assemble batteries, and their electrochemical performance was tested. The specific steps are as follows:

[0146] (1) Slurry preparation: Weigh the negative electrode material, conductive agent and binder in a ratio of 8:1:1, add solvent water to adjust the viscosity of the slurry, and stir for 3 to 5 hours.

[0147] (2) Coating: The slurry is coated onto the copper foil current collector using a scraper mold.

[0148] (3) Drying: Dry in a vacuum drying oven at 120°C for 12 hours.

[0149] (4) Cutting: Cut into circular negative electrode sheets with a diameter of 15mm, weigh them and place them in a drying oven.

[0150] (5) Assembly: In the glove box, CR2025 button cells are assembled using lithium sheets as the counter electrode.

[0151] The electrolyte was a 1M LiPF6 / EC:DMC (1:1, vol) mixture, and the diaphragm was a Celgard 2300 polypropylene microporous membrane.

[0152] The sealed battery was left to stand for 24 hours, and then charge-discharge and cycle performance tests were conducted using the Land battery performance testing system. The test results are listed in Table 2 below.

[0153] Table 2

[0154]

[0155]

[0156] As can be seen from the data in the table above, compared with the products obtained in Comparative Examples 1 to 3, the pre-lithiated silicon-based composite material A1 obtained in Example 1 using the preparation method of this disclosure can have higher initial coulombic efficiency and capacity retention in lithium-ion battery anode material applications.

[0157] Furthermore, a comparison of the examples with Comparative Example 1 shows that Comparative Example 1 did not add sodium carboxymethyl cellulose and pitch during spray drying, and the resulting product D-1 had bubble generation during homogenization, while A-1 prepared by the method of this disclosure can avoid bubble generation during homogenization.

[0158] Furthermore, comparing the products obtained in Example 1 and Example 3, it can be seen that the thermal stabilization sintering process conditions in Example 3 meet the preferred embodiment of this disclosure, and the pre-lithiated silicon-based composite material A3 obtained therefrom can have a higher first coulombic efficiency in the application of lithium-ion battery anode materials.

[0159] Comparing the products obtained in Example 1 and Example 4, it can be seen that the spray granulation process conditions in Example 4 meet the preferred embodiment of this disclosure, and the pre-lithiated silicon-based composite material A4 obtained therefrom can have a higher first coulombic efficiency in the application of lithium-ion battery anode materials.

[0160] Comparing the products obtained in Example 1 and Example 5, it can be seen that the pre-lithiated silicon-based composite material A1 obtained in Example 1, which uses a two-stage sintering process, can have higher initial coulombic efficiency and cycle capacity retention in lithium-ion battery anode material applications.

[0161] Comparing the products obtained in Example 1 and Example 6, it can be seen that the weight ratio of materials added during the preparation process in Example 6 meets the preferred embodiment of this disclosure, and the pre-lithiated silicon-based composite material A6 obtained therefrom can have a higher first coulombic efficiency in the application of lithium-ion battery anode materials.

[0162] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0163] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0164] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method for preparing a pre-lithiated silicon-based composite material, characterized in that, The method includes the following steps: S1. Mix lithium metal with porous silicon-based material powder, and then perform solid-phase homogenization treatment to obtain the first mixture. S2. Add the solid dispersant to the first mixture and perform dispersion and homogenization treatment to obtain the second mixture; S3. The carbonizable organic carbon source binder, solvent and the second mixture are mixed and homogenized to obtain a mixed slurry; S4. The mixed slurry is subjected to spray granulation treatment to obtain a pre-lithiated composite material precursor; S5. The pre-lithiated composite material precursor is subjected to sintering treatment; The above steps S1 to S5 are carried out in an inert atmosphere.

2. The method according to claim 1, characterized in that, In step S1, the porous silicon-based material powder has an average particle size of 0.5~10μm, an average pore size of 0.5~30nm, and a BET specific surface area of ​​0.1~100m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g; The lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powder, or lithium sheets.

3. The method according to claim 1, characterized in that, In step S1, the weight ratio of the lithium metal to the porous silicon-based material powder is 1:(1~100).

4. The method according to claim 1, characterized in that, In step S1, the weight ratio of the lithium metal to the porous silicon-based material powder is 1:(5~50).

5. The method according to claim 1, characterized in that, Before step S1, the method further includes: The silicon alloy raw material is acid-etched, then washed and dried to obtain the porous silicon-based material powder.

6. The method according to claim 5, characterized in that, The silicon alloy is selected from one or more of silicon-aluminum alloy, silicon-iron alloy and silicon-magnesium alloy; the silicon content in the silicon alloy raw material is 30-70% by weight.

7. The method according to claim 1, characterized in that, In step S1, the solid phase homogenization process includes mechanical homogenization, which is selected from any one of ball mill, sand mill, homogenizer or disperser.

8. The method according to claim 1, characterized in that, In step S1, the rotation speed of the solid phase homogenization treatment is 300~2000 r / min, the homogenization time is 6~72 h, and the ball-to-material ratio is (1~30):

1.

9. The method according to claim 1, characterized in that, In step S2, the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, and soft carbon; The weight ratio of the solid dispersant to the lithium metal is (1~50):

1.

10. The method according to claim 9, characterized in that, The weight ratio of the solid dispersant to the lithium metal is (5~10):

1.

11. The method according to claim 1, characterized in that, In step S2, the dispersion and homogenization process includes mechanical homogenization, which is selected from any one of ball mill, sand mill, homogenizer or disperser; The dispersion and homogenization process is carried out at a rotation speed of 50~500 r / min for 0.5~12 h, with a ball-to-material ratio of (1~50):

1.

12. The method according to claim 1, characterized in that, In step S3, the organic carbon source binder is selected from one or more of polymer carbon sources, petroleum-based carbon sources, sugar carbon sources, and other carbon sources; The polymer carbon source includes one or more of phenolic resin, epoxy resin, polyvinylpyrrolidone, and polyvinyl alcohol; The petroleum-based carbon sources include one or more of pitch, petroleum coke and needle coke; The carbohydrate carbon source includes one or more of glucose, sucrose, and fructose; The other carbon source is selected from one or two of sodium carboxymethyl cellulose and carboxylated styrene-butadiene latex; the solvent is selected from one or more of ethanol, isopropanol, n-butanol, cyclohexane and cyclohexanone.

13. The method according to claim 1, characterized in that, In step S3, the weight ratio of the organic carbon source binder to metallic lithium is (10~100):1; The weight ratio of the solvent to the organic carbon source adhesive is (10~50):

1.

14. The method according to claim 13, characterized in that, The weight ratio of the organic carbon source binder to metallic lithium is (40~80):

1.

15. The method according to claim 1, characterized in that, In step S4, the conditions for spray granulation include: inlet temperature of 100~300℃, outlet temperature of 50~200℃, carrier gas flow rate of 10~100 L / min, and pressure of -0.1 to -0.08MPa.

16. The method according to claim 15, characterized in that, In step S4, the conditions for spray granulation include: inlet temperature of 120~240℃, outlet temperature of 80~150℃, carrier gas flow rate of 30~60L / min, and pressure of -0.1 to -0.05MPa.

17. The method according to claim 1, characterized in that, In step S5, the sintering process includes a first-stage sintering and a second-stage sintering; wherein the temperature of the first-stage sintering is 200~500℃, the heating rate is 1~3℃ / min, and the holding time is 1~6h; the temperature of the second-stage sintering is 500~1200℃, the heating rate is 1~5℃ / min, and the holding time is 1~12h.

18. The method according to claim 17, characterized in that, The first sintering temperature is 250~400℃, the heating rate is 2~3℃ / min, and the holding time is 2~3h; the second sintering temperature is 700~900℃, the heating rate is 2~3℃ / min, and the holding time is 2~6h.

19. The method according to claim 1, characterized in that, The inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton, and xenon; the water content and oxygen content of the inert atmosphere are less than 0.1% by weight and less than 0.1% by weight.

20. The method according to claim 1, characterized in that, The pre-lithiated silicon-based composite material prepared by this method comprises pre-lithiated silicon-based composite particles with a core-shell structure. The core of the pre-lithiated silicon-based composite particles comprises a porous silicon matrix and a core lithium-containing component dispersed on the surface and in the pores of the silicon matrix. The outer surface of the core is covered with a first carbon layer and a second carbon layer from the inside out, and the first carbon layer and the second carbon layer form the outer shell of the core-shell structure.

21. The method according to claim 20, characterized in that, The first carbon layer contains a first lithium-containing component, and the second carbon layer is lithium-free.

22. The method according to claim 21, characterized in that, The lithium content in the core is greater than the lithium content in the first carbon layer.

23. The method according to claim 21, characterized in that, The core lithium-containing component comprises one or more of lithium silicon alloy, lithium silicate, and lithium oxide; the first lithium-containing component comprises one or more of lithium carbide, lithium silicate, and lithium oxide.

24. The method according to claim 20, characterized in that, The total thickness of the first carbon layer and the second carbon layer is 10~1000nm.

25. The method according to claim 24, characterized in that, The thickness of the first carbon layer is 10~500nm, and the thickness of the second carbon layer is 5~500nm.

26. The method according to claim 20, characterized in that, The pre-lithiated silicon-based composite particles have an average particle size of 0.5–30 μm, an average pore size of 1–30 nm, and a BET specific surface area of ​​0.5–50 m². 2 / g, total pore volume is 0.005~0.5cm³ 3 / g.

Citation Information

Patent Citations

  • Method for producing negative electrode active material for nonaqueous electrolyte secondary batteries and method for producing negative electrode for nonaqueous electrolyte secondary batteries

    CN109075330A

  • Preparation method of pre-lithium alloy with porous structure

    CN110224122A

  • Silicon-based negative electrode material and preparation method and application thereof