Silicon monoxide-based lithia supplementing additive, preparation method thereof, negative electrode composite material, negative electrode and battery

By using a silicon suboxide-based lithium supplementation additive to generate lithium silicate and lithium oxide in lithium-ion batteries, the volume expansion is buffered and lithium ions are replenished, solving the volume expansion problem of silicon materials, improving coulombic efficiency and cycle stability, reducing costs, and making it suitable for aqueous homogenization environments.

CN117747977BActive Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211131744.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2026-11-20
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

The existing silicon anode material for lithium-ion batteries suffers from volume expansion during lithium insertion/extraction, leading to pulverization and shedding, consuming Li⁺, reducing coulombic efficiency and cycle performance. Furthermore, existing lithium replenishment methods pose safety hazards and high costs in aqueous slurry environments.

Method used

A silicon suboxide-based lithium supplement additive is used to mix metallic lithium with silicon suboxide through a solid-phase homogenization reaction to generate lithium silicate and lithium oxide. This buffers volume expansion and replenishes lithium ions during charge-discharge cycles. Solid dispersants are used to avoid agglomeration, making it suitable for aqueous homogenization environments.

Benefits of technology

It improves the initial coulombic efficiency and cycle stability of lithium-ion batteries, reduces production costs, is easy to operate, is applicable to existing lithium-ion battery anode material systems, and features controllable lithium content, environmental friendliness, and ease of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117747977B_ABST
    Figure CN117747977B_ABST
Patent Text Reader

Abstract

The present disclosure relates to a silicon monoxide-based lithium supplement additive, a preparation method thereof, a negative electrode composite material, a negative electrode and a battery, the method comprising the following steps: (1) mixing metallic lithium with silicon monoxide powder under an inert atmosphere, and then performing solid-phase homogenization reaction to obtain a reaction mixture; (2) mixing the reaction mixture with a solid dispersant under an inert atmosphere, and then performing dispersion homogenization treatment. The silicon monoxide-based lithium supplement additive is suitable for a water-based homogenization environment of a lithium ion battery, and can effectively improve the first coulomb efficiency and cycle stability of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of lithium-ion batteries, specifically to a silicon suboxide-based lithium supplementation additive and its preparation method, a negative electrode composite material, a negative electrode, and a battery. Background Technology

[0002] Among novel anode materials, silicon has attracted widespread attention due to its advantages such as high theoretical capacity, abundant reserves, and low discharge voltage when used in battery anodes. However, silicon suffers from volume expansion (>300%) during the lithium insertion / extraction process in lithium-containing batteries, which can easily lead to pulverization and detachment of the anode material, ultimately causing the anode material to lose electrical contact and resulting in battery failure. Furthermore, the repeated volume expansion and contraction of silicon continuously damages the surface SEI film, constantly consuming the Li₂ of the cathode. + This reduces the battery's coulombic efficiency, which in turn leads to a deterioration in the battery's cycle performance and affects its lifespan.

[0003] Pre-lithiation technology can solve the problem of irreversible capacity loss, improve coulombic efficiency, and enhance cycle stability in lithium-ion batteries. Currently, there are two main methods for lithium replenishment in negative electrodes. First, pure lithium powder is directly added to the negative electrode. For example, FMC in the US developed Stabilized Lithium Metal Powder (SLMP) for pre-lithiation of negative electrodes (Chinese patents CN101790806A and CN103447541). This involves dripping a toluene solution containing SLMP onto the negative electrode surface, pressing the sheet after solvent evaporation, crushing the passivation layer on the SLMP particles, and exposing the lithium metal to replenish the electrolyte, thus improving the pre-lithiation effect. This method results in highly active lithium sheets that are difficult to process and cannot guarantee uniform distribution of lithium powder, leading to serious safety hazards in the resulting lithium batteries. Second, the surface of a highly active lithium source is modified and passivated, then mixed uniformly with the negative electrode material through a slurry method for lithium replenishment. This method ensures material uniformity, is easy to operate, and also guarantees a certain degree of battery safety. As disclosed in CN103779572A, a polymer passivation layer is coated on the surface of lithium powder, which can be mixed evenly with the negative electrode material in an oily medium.

[0004] However, the aforementioned lithium-replenishing additives are all limited to oily media, which contradicts the actual aqueous slurry environment used in current lithium battery anode production. The use of oily media undoubtedly increases production costs. Therefore, developing a highly efficient aqueous lithium-replenishing additive for anodes has significant practical application value. Summary of the Invention

[0005] The purpose of this disclosure is to provide a silicon suboxide-based lithium supplement additive and its preparation method, a negative electrode composite material, a negative electrode, and a battery. This silicon suboxide-based lithium supplement additive is suitable for use in aqueous slurry environments for lithium-ion batteries and can effectively improve the initial coulombic efficiency and cycle stability of lithium-ion batteries.

[0006] To achieve the above objectives, the first aspect of this disclosure provides a method for preparing a silicon suboxide-based lithium supplementation additive, the method comprising the following steps: (1) mixing lithium metal with silicon suboxide powder under an inert atmosphere and then performing a solid-phase homogenization reaction to obtain a reaction mixture; (2) mixing the reaction mixture with a solid dispersant under an inert atmosphere and then performing a dispersion homogenization treatment.

[0007] Optionally, the method further includes: sealing the material obtained in step (2) under an inert atmosphere to obtain a silicon suboxide-based powder lithium supplementation additive.

[0008] Optionally, in step (1), the weight ratio of the silicon suboxide powder to the lithium metal is (1-200):1, preferably (10-50):1.

[0009] Optionally, the median particle size of the silica powder is 1–20 μm, preferably 1–5 μm; the average pore size is 1–50 nm, preferably 5–20 nm; and the BET specific surface area is 0.5–100 m². 2 / g, preferably 0.5~10m 2 / g, total pore volume is 0.001~0.5cm³ 3 / g, preferably 0.001~0.1cm 3 / g; Optionally, the chemical formula of the silica powder is SiO2. x Where 0.5≤x<2; the lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powders or lithium sheets.

[0010] Optionally, in step (1), the solid-phase homogenization reaction includes mechanical homogenization, which is selected from any one of ball mill, sand mill, homogenizer or disperser; Optionally, in step (1), the solid-phase homogenization reaction conditions include: rotation speed of 200-1000 r / min, homogenization time of 2-48 h, homogenization temperature of 25-200 °C, and ball-to-material ratio of (1-30):1; Preferably, the rotation speed is 450-800 r / min, homogenization time is 10-24 h, homogenization temperature is 50-100 °C, and ball-to-material ratio is (20-30):1.

[0011] Optionally, in step (2), the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon and soft carbon; the weight ratio of the solid dispersant to the lithium metal is (0.1-2):1, preferably (0.1-0.5):1.

[0012] Optionally, in step (2), the dispersion and homogenization process includes mechanical homogenization, which is selected from any one of ball mill, sand mill, homogenizer or disperser; Optionally, in step (2), the conditions for dispersion and homogenization include: rotation speed of 100-450 r / min, time of 0.5-12 h, temperature of 25-200 °C, and ball-to-material ratio of (1-30):1; Preferably, the rotation speed is 100-300 r / min, homogenization time is 1-5 h, homogenization temperature is 50-100 °C, and ball-to-material ratio is (20-30):1.

[0013] Optionally, in steps (1) and (2), the inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton and xenon; the water content of the inert atmosphere is less than 0.1% by weight and the oxygen content is less than 0.1% by weight.

[0014] The second aspect of this disclosure provides a silicon suboxide-based lithium supplement additive prepared using the method provided in the first aspect of this disclosure.

[0015] A third aspect of this disclosure provides a silicon suboxide-based lithium supplement additive, the silicon suboxide-based lithium supplement additive comprising silicon suboxide-based lithium supplement particles and a solid dispersant; the silicon suboxide-based lithium supplement particles comprising a silicon suboxide matrix and a lithium-containing component, the lithium-containing component being dispersed on the surface and / or within clusters of the silicon suboxide matrix; the lithium-containing component comprising one or more of lithium silicate, lithium oxide, lithium, and lithium silicides.

[0016] Optionally, the weight ratio of silicon suboxide-based lithium supplementation particles to solid dispersant in the silicon suboxide-based lithium supplementation additive is (10-60):1, preferably (20-55):1; preferably, the content of the lithium-containing component is 0.01-50% by weight, preferably 0.9-20% by weight, based on the total weight of the silicon suboxide-based lithium supplementation particles; optionally, the silicon suboxide-based lithium supplementation particles further contain elemental silicon, which is dispersed on the surface and / or within the clusters of the silicon suboxide matrix; optionally, the silicon suboxide-based lithium supplementation particles are diffusely dispersed in the solid dispersant; optionally, the solid dispersant includes one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, and soft carbon.

[0017] Optionally, the median particle size of the silicon suboxide-based lithium replenishing particles is 0.1–5 μm, preferably 0.1–1.5 μm; the average pore size is 1–50 nm, preferably 10–30 nm; and the BET specific surface area is 0.1–100 m². 2 / g, preferably 1-35m 2 / g; total pore volume is 0.001~0.5cm³ 3 / g, preferably 0.05~0.2cm 3 / g.

[0018] The fourth aspect of this disclosure provides a negative electrode composite material, the negative electrode composite material comprising the silicon suboxide-based lithium supplementation additive described in the third aspect of this disclosure.

[0019] Optionally, the negative electrode material further comprises a negative electrode host material; wherein the negative electrode host material is selected from one or more of silicon suboxide negative electrode materials, graphite negative electrode materials and silicon-carbon negative electrode materials; optionally, the weight ratio of the negative electrode host material to the silicon suboxide-based lithium supplementation additive is (1-50):1, preferably (1-10):1.

[0020] Optionally, the negative electrode composite material is prepared by a method including the following steps: mixing the negative electrode host material with the silicon suboxide-based lithium supplementation additive.

[0021] The fifth aspect of this disclosure provides a negative electrode comprising the negative electrode composite material described in the fourth aspect of this disclosure.

[0022] A sixth aspect of this disclosure provides a lithium-ion battery including the negative electrode described in the fifth aspect of this disclosure.

[0023] Through the above technical solutions, this disclosure provides a silicon suboxide-based lithium replenishment additive and its preparation method, a negative electrode composite material, a negative electrode, and a battery. This disclosure uses silicon suboxide and metallic lithium as raw materials, achieving lithium introduction through a solid-phase homogeneous reaction. A portion of the metallic lithium reacts with oxygen in the silicon suboxide to generate lithium silicate and lithium oxide, which solves the problem of reduced initial coulombic efficiency of silicon suboxide itself. Simultaneously, it acts as a buffer medium to buffer volume expansion during cycling, making the material structure more stable. Another portion of the metallic lithium remains in the silicon suboxide clusters, replenishing lithium during charge-discharge cycles, compensating for lithium-ion consumption and loss during battery cycling, and improving capacity cycle stability. Furthermore, this disclosure further avoids silicon suboxide-lithium agglomeration and adhesion by subsequently introducing a solid dispersant. The silicon suboxide-based lithium replenishment additive provided by this disclosure is suitable for aqueous slurry environments in lithium battery negative electrode production, eliminating the need for oily media and reducing costs. It can also be directly mixed with existing lithium-ion battery negative electrode materials, simplifying operation and facilitating industrial-scale application, effectively improving the initial coulombic efficiency and cycle stability of lithium-ion batteries. The preparation method disclosed herein is a solid-phase homogeneous reaction method, which is compatible with existing lithium-ion battery anode materials and assembly systems, and can be directly applied to existing lithium-ion battery anode material systems; at the same time, it has the characteristics of controllable lithium content, simple process, easy operation, environmentally friendly process, low cost, and is conducive to large-scale production.

[0024] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0025] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings:

[0026] Figure 1 A schematic diagram of the structure of the silicon suboxide-based lithium supplementary additive provided in this disclosure;

[0027] Figure 2 Scanning electron microscope (SEM) images of the product prepared in Example 1;

[0028] Figure 3 The X-ray diffraction pattern of the product prepared in Example 1;

[0029] Figure 4 Transmission electron microscope (TEM) image of the product prepared in Example 1;

[0030] Figure 5 The high-resolution X-ray photoelectron spectroscopy (XPS) of the product prepared in Example 1 is shown below.

[0031] Figure 6The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of the product prepared in Example 1;

[0032] Figure 7 To test the cycle performance of the battery in Example 2, which used the product obtained in Example 1 directly as the negative electrode material, at a current density of 0.2C;

[0033] Figure 8 To test the rate performance of the battery in Example 2, which uses the product obtained in Example 2 directly as the negative electrode material, at a current density of 0.2C;

[0034] Figure 9 To test the cycle performance of the battery in Comparative Example 1, which uses silicon suboxide powder directly as the negative electrode material, at a current density of 0.2C. Detailed Implementation

[0035] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.

[0036] The first aspect of this disclosure provides a method for preparing a silicon suboxide-based lithium supplementation additive, the method comprising the following steps:

[0037] (1) Under an inert atmosphere, lithium metal and silicon suboxide powder are mixed and subjected to a solid-phase homogeneous reaction to obtain a reaction mixture.

[0038] (2) Under an inert atmosphere, the reaction mixture is mixed with a solid dispersant and then subjected to dispersion and homogenization treatment.

[0039] This disclosure provides a method for preparing a silicon suboxide-based lithium replenishment additive. Using silicon suboxide and lithium metal as raw materials, lithium is introduced through a solid-phase homogeneous reaction. A portion of the lithium metal reacts with oxygen in the silicon suboxide to form lithium silicate and lithium oxide, which solves the problem of reduced initial coulombic efficiency of silicon suboxide itself. Simultaneously, it acts as a buffer medium to buffer volume expansion during cycling, making the material structure more stable. Another portion of the lithium metal remains in the silicon suboxide material to replenish lithium during charge-discharge cycles, compensating for lithium-ion consumption and loss during battery cycling, and improving capacity cycle stability. Furthermore, this disclosure further avoids silicon suboxide-lithium agglomeration and adhesion by subsequently introducing a solid dispersant. The silicon suboxide-based lithium replenishment additive provided by this disclosure is suitable for aqueous slurry environments in lithium battery anode production, eliminating the need for oil-based media and reducing costs. It can also be directly mixed with existing lithium-ion battery anode materials, simplifying operation and facilitating industrial-scale application, effectively improving the initial coulombic efficiency and cycle stability of lithium-ion batteries. The preparation method disclosed herein is a solid-phase homogeneous reaction method, which is compatible with existing lithium-ion battery anode materials and assembly systems, and can be directly applied to existing lithium-ion battery anode material systems; at the same time, it has the characteristics of controllable lithium content, simple process, easy operation, environmentally friendly process, low cost, and is conducive to large-scale production.

[0040] In one embodiment, the method further includes: sealing the material obtained in step (2) under an inert atmosphere to obtain a silicon suboxide-based powder lithium supplement additive. This disclosure effectively protects the activity of the silicon suboxide-based powder lithium supplement additive by sealing and storing the obtained product under an inert atmosphere, preventing contact with substances such as moisture and oxygen in the air; the powder form of the silicon suboxide-based lithium supplement additive provided by this disclosure is also easy to store and facilitates wider application.

[0041] In one embodiment, in step (1), the weight ratio of the silicon suboxide powder to lithium metal is (1-200):1, preferably (10-50):1. This weight ratio in this embodiment results in a better homogeneous reaction between the silicon suboxide powder and lithium metal, leading to improved coulombic efficiency and cycle stability when the resulting lithium-ion additive is applied to lithium-ion batteries.

[0042] In one embodiment, the median particle size of the silica powder is 1–20 μm, preferably 1–5 μm; the average pore size is 1–50 nm, preferably 5–20 nm; and the BET specific surface area is 0.5–100 m². 2 / g, preferably 0.5~10m 2 / g, total pore volume is 0.001~0.5cm³ 3 / g, preferably 0.001~0.1cm 3 / g.

[0043] In one embodiment, the chemical formula of the silica powder is SiO₂. x Where 0.5 ≤ x < 2. In this disclosure, silicon suboxide powder SiO x The value of "x" is obtained based on the oxygen content test method.

[0044] In one embodiment, the lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powder, or lithium sheets.

[0045] In one embodiment, in step (1), the solid-phase homogenization reaction is carried out by mechanical homogenization, wherein the mechanical homogenization is selected from any one of ball mill, sand mill, homogenizer or disperser.

[0046] In a preferred embodiment, the conditions for the solid-phase homogenization reaction in step (1) include: a rotation speed of 200–1000 r / min, a homogenization time of 6–72 h, a homogenization temperature of 25–200 °C, and a ball-to-material ratio of (1–20):1. The solid-phase homogenization reaction provided in this disclosure is simple to operate and can effectively introduce lithium into silica powder.

[0047] In a preferred embodiment, the conditions for the solid-phase homogenization reaction in step (1) include: a rotation speed of 450–800 r / min, a homogenization time of 10–24 h, a homogenization temperature of 50–100 °C, and a ball-to-material ratio of (20–30):1. Performing the solid-phase homogenization reaction under these preferred conditions according to this embodiment can further improve the performance of the additive.

[0048] In one embodiment, in step (2), the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon and soft carbon;

[0049] The weight ratio of the solid dispersant to the lithium metal is (0.1-2):1, preferably (0.1-0.5):1.

[0050] In this disclosure, a solid dispersant is added during the preparation process, which allows the homogeneous solid reaction product to be dispersed in the solid dispersant. This effectively prevents the agglomeration of silicon suboxide and lithium metal during the ball milling reaction, ensuring that the silicon suboxide-lithium particles are fully dispersed. At the same time, the solid dispersant can also form a diffusely distributed conductive network, increasing the conductivity of the particles and suppressing the decrease in conductivity caused by the introduction of lithium.

[0051] In one embodiment, the conditions for the dispersion and homogenization treatment in step (2) include: rotation speed of 100-450 r / min, time of 0.5-12 h, temperature of 25-200 °C, and ball-to-material ratio of (1-30):1.

[0052] In a preferred embodiment, the conditions for the dispersion and homogenization process in step (2) include: rotation speed of 100-300 r / min, homogenization time of 1-5 h, homogenization temperature of 50-100 °C, and ball-to-material ratio of (20-30):1.

[0053] In one embodiment, in steps (1) and (2), the inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton, and xenon; the water content and oxygen content of the inert atmosphere are less than 0.1% by weight and less than 0.1% by weight. In the above embodiment, the use of a preferred inert gas environment can further prevent lithium from reacting with oxygen and water in the environment, making the material structure more stable.

[0054] According to this disclosure, the method for preparing silicon suboxide-based lithium supplement additives further includes: sealing and storing the uniformly dispersed silicon suboxide-based lithium supplement additives in an inert atmosphere.

[0055] The second aspect of this disclosure provides a silicon suboxide-based lithium supplementation additive prepared according to the method described in the first aspect of this disclosure.

[0056] A third aspect of this disclosure provides a silicon suboxide-based lithium supplement additive, the silicon suboxide-based lithium supplement additive comprising silicon suboxide-based lithium supplement particles and a solid dispersant; the silicon suboxide-based lithium supplement particles comprising a silicon suboxide matrix and a lithium-containing component, the lithium-containing component being dispersed on the surface and / or within clusters of the silicon suboxide matrix; the lithium-containing component comprising one or more of lithium silicate, lithium oxide, lithium, and lithium silicides.

[0057] The silicon suboxide-based lithium supplement additive disclosed herein introduces one or more of lithium silicate, lithium oxide, lithium metal, and lithium silicate into the silicon suboxide-based powder, effectively improving the initial coulombic efficiency and cycle stability of lithium-ion batteries.

[0058] In a further embodiment, the silicon suboxide-based lithium supplement particles further comprise elemental silicon, which is dispersed on the surface and / or within the clusters of the silicon suboxide matrix.

[0059] According to this disclosure, lithium silicate is a product of the chemical formula Li x SiO y It is indicated that the specific chemical composition may include one or more of Li2Si2O5, Li2SiO3 and Li4SiO4.

[0060] According to this disclosure, the chemical composition of the lithium silicate in the silicon suboxide-based lithium replenishment particles can be entirely Si₂Li₂O₅. Si₂Li₂O₅ has a relatively stable thermodynamic structure and good water resistance. During the material slurry coating process, it will not cause an increase in the pH of the slurry. During battery cycling, it can reduce the consumption and loss of lithium ions. Simultaneously, as a buffer medium, it can buffer the volume expansion during cycling, making the material structure more stable. According to this disclosure, the chemical composition of the lithium silicate is obtained by controlling the weight ratio of silicon suboxide powder to metallic lithium.

[0061] In one embodiment, the weight ratio of silicon suboxide-based lithium supplementation particles to solid dispersant in the silicon suboxide-based lithium supplementation additive is (10-60):1, preferably (20-55):1.

[0062] In one embodiment, the silicon suboxide-based lithium supplement additive comprises 50-99% by weight of silicon suboxide-based lithium supplement particles and 1-50% by weight of a solid dispersant. In a preferred embodiment, the silicon suboxide-based lithium supplement additive comprises 80-90% by weight of silicon suboxide-based lithium supplement particles and 1-10% by weight of a solid dispersant.

[0063] In one embodiment, the lithium-containing component content is 0.01 to 50% by weight, preferably 0.9 to 20% by weight, based on the total weight of the silicon suboxide-based lithium supplement particles.

[0064] In one specific embodiment, the silicon suboxide-based lithium supplement particles are diffusely dispersed in the solid dispersant. The dispersion of the silicon suboxide-based lithium supplement particles can be observed using scanning electron microscopy (SEM) images.

[0065] In one embodiment, the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, and soft carbon.

[0066] In one embodiment, the median particle size of the silicon suboxide-based lithium replenishing particles is 0.1–5 μm, preferably 0.1–1.5 μm; the average pore size is 1–50 nm, preferably 10–30 nm; and the BET specific surface area is 0.1–100 m². 2 / g, preferably 1-35m 2 / g; total pore volume is 0.001~0.5cm³ 3 / g, preferably 0.05~0.2cm 3 / g.

[0067] The fourth aspect of this disclosure provides a negative electrode composite material comprising the silicon suboxide-based lithium supplementation additive described in the second or third aspect of this disclosure.

[0068] In one specific embodiment, the negative electrode composite material further comprises a negative electrode host material; the negative electrode host material is selected from one or more of silicon suboxide negative electrode materials, graphite negative electrode materials, and silicon-carbon negative electrode materials. In this disclosure, lithium-ion battery negative electrode materials known in the art can be used as the negative electrode host material, and these materials are readily available. The negative electrode host material can be obtained through ordinary commercial channels or prepared using methods known in the art. For example, the composition of the silicon suboxide negative electrode material can be SiO₂. x 0 <x<2。

[0069] In a preferred embodiment, the weight ratio of the negative electrode substrate material to the silicon suboxide-based lithium supplementation additive is (1-50):1, preferably (1-10):1.

[0070] The negative electrode composite material disclosed herein can be used in combination with existing negative electrode materials through simple operation, and can also effectively improve the first coulombic efficiency and cycle stability of lithium-ion batteries, and has good compatibility with existing battery systems.

[0071] In one specific embodiment, the negative electrode composite material is prepared by a method including the following steps: mixing the negative electrode host material with the silicon suboxide-based lithium supplementation additive.

[0072] The fifth aspect of this disclosure provides a negative electrode comprising the silicon suboxide-based lithium supplementation additive described in the second or third aspect of this disclosure, or the negative electrode composite material described in the fourth aspect of this disclosure.

[0073] According to this disclosure, the negative electrode can be prepared using conventional processes in the art.

[0074] In one specific embodiment, the negative electrode is prepared by a method including the following steps:

[0075] (1) Slurry preparation: Weigh the negative electrode composite material, conductive agent and binder at a ratio of (7-8.9):(0.1-2):1, add solvent water to adjust the viscosity of the slurry, and stir for 3-5 hours; the conductive agent and binder can be materials conventionally selected in this field;

[0076] (2) Coating: The slurry is coated onto the copper foil current collector using a doctor blade mold;

[0077] (3) Drying: Dry in a vacuum drying oven at 80-150℃ for 6-48 hours;

[0078] (4) Cutting: Cut into negative electrode sheets for batteries, weigh them and place them in a drying oven.

[0079] The sixth aspect of this disclosure provides a lithium-ion battery comprising the silicon suboxide-based lithium supplementation additive described in the second or third aspect of this disclosure, or the negative electrode composite material described in the fourth aspect of this disclosure, or the negative electrode described in the fifth aspect of this disclosure.

[0080] In one specific embodiment, the lithium-ion battery provided in this disclosure uses the negative electrode provided in the fifth aspect mentioned above, and uses a lithium sheet as the counter electrode; uses a 0.5-1M LiPF6 / EC:DMC (0.5-1:1, vol) mixture as the electrolyte; and uses a polypropylene microporous membrane as the separator, and assembles and seals to obtain the lithium-ion battery.

[0081] The present disclosure will be further illustrated by the following examples, but the present disclosure is not limited thereto.

[0082] Unless otherwise specified, all raw materials used in the following embodiments are commercially available products.

[0083] In the following embodiments, the specific testing methods are as follows:

[0084] The median particle size was measured using a Mastersizer 3000 optical particle size analyzer.

[0085] The average pore size, BET specific surface area, and total pore volume were measured using a specific surface area and pore size analyzer JW-BK100.

[0086] The SEM testing method was a scanning electron microscope, and the instrument model was Hitachi S4800 from Japan.

[0087] The TEM test method was transmission electron microscopy, and the instrument model was Hitachi FEI G2F20 from Japan.

[0088] The XRD test method was an X-ray diffractometer, specifically the PANalytical X'Pert PRO powder X-ray diffractometer.

[0089] The XPS test method is X-ray photoelectron spectroscopy, and the instrument model is VG ESCALAB;

[0090] The electrochemical cycling performance was tested using the Blue Electricity testing system, instrument model CT3001A.

[0091] In the following examples and comparative examples, commercially available silica powder with a median particle size of 2–10 μm and an average pore size of 1–50 nm was used; the BET specific surface area was 0.5–100 m². 2 / g; total pore volume is 0.001~0.5cm³ 3 / g; the chemical formula of the silica suboxide powder is SiO2 x, where 0.5≤x<2.

[0092] Example 1

[0093] Under an anhydrous and oxygen-free inert environment, 2g of silicon suboxide and 0.02g of lithium metal ingot (the weight ratio of silicon suboxide powder to lithium metal is 100:1) were weighed and placed in a zirconia ball mill jar. After sealing, the jar was transferred to a planetary ball mill for ball milling. The ball-to-material ratio was 20:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The milling was carried out at 50°C, with a milling speed of 500 rpm for 12 hours. Then, 0.1g of natural graphite was added and ball milling continued (the weight ratio of solid dispersant to lithium metal was 5:1). The milling was carried out at 50°C, with a milling speed of 450 rpm for 2 hours. The powder was then removed and sealed in an anhydrous and oxygen-free inert environment for storage, yielding a silicon suboxide-based lithium supplementary powder, denoted as T-1.

[0094] Figure 2 The image shows a SEM image of the silicon suboxide-based lithium supplement additive T-1. As can be seen from the image, the silicon suboxide-based powder lithium supplement additive T-1 prepared in this embodiment is granular with good dispersibility, an average particle size of 0.5-2 μm, and a relatively smooth surface structure.

[0095] Figure 3 The X-ray diffraction pattern of silicon suboxide-based lithium supplement additive T-1 is shown. The pattern reveals that the main component of the silicon suboxide-based powder lithium supplement additive T-1 remains amorphous silicon suboxide.

[0096] Figure 4 TEM image of T-1, a lithium supplement additive based on silicon suboxide. The image shows distinct lithium silicates, lithium-silicon alloys, and characteristic lattice fringes of silicon, indicating that lithium was successfully introduced into silicon suboxide and partially reduced Si. Some Li reacted with oxygen in silicon suboxide to form lithium silicates, while some Li reacted with Si to form lithium-silicon alloys.

[0097] Figure 5 The Si 2p X-ray photoelectron high-resolution scanning energy spectrum of silicon suboxide-based lithium supplement T-1 was obtained from... Figure 5 It can be seen that significant Si content was observed in the silicon suboxide-based lithium supplement additive T-1. 0 (98.7eV) and Si 4+ Characteristic peak (102.4 eV); Figure 6 The Li 1s X-ray photoelectron high-resolution scanning energy spectrum of silicon suboxide-based lithium supplement T-1 was obtained from... Figure 6 It can be seen that a sharp characteristic peak of Li appeared in the silicon suboxide-based lithium supplement T-1, which further indicates that lithium was introduced into the silicon suboxide group.

[0098] Comparative Example 1

[0099] The preparation method is similar to that of Example 1, except that lithium metal is not added. Specifically, the following steps are included:

[0100] 2g of silicon suboxide was weighed and placed in a zirconia ball mill jar. After sealing, it was transferred to a planetary ball mill for ball milling. The ball-to-material ratio was 20:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The milling was carried out at 50℃, with a milling speed of 500 rpm for 12 hours. Then, 0.1g of natural graphite was added and ball milling continued (the weight ratio of solid dispersant to lithium metal was 5:1). The milling was carried out at 50℃, with a milling speed of 450 rpm for 2 hours. The powder was removed and sealed in an inert environment free of water and oxygen, and stored to obtain a lithium-free silicon suboxide-based additive, denoted as DT-1.

[0101] Comparative Example 2

[0102] The preparation method is similar to that of Example 1, except that no solid dispersant is added. Specifically, the following steps are included:

[0103] Weigh 2g of silicon suboxide and 0.02g of lithium metal ingot (the weight ratio of silicon suboxide powder to lithium metal is 100:1) and place them in a zirconia ball mill jar. After sealing, transfer the jar to a planetary ball mill for ball milling. The ball-to-material ratio is 20:1, and the zirconia balls have diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The milling temperature is 50℃, the milling speed is 500 rpm, and the milling time is 12 hours. The extracted powder is labeled DT-2.

[0104] Comparative Example 3

[0105] The preparation method is similar to that of Example 1, except that:

[0106] Weigh 5g of silicon suboxide and 0.02g of lithium metal ingot (the weight ratio of silicon suboxide powder to lithium metal is 250:1). The rest of the preparation process is the same as in Example 1, and a silicon-based powder lithium supplement additive is obtained, which is denoted as DT-3.

[0107] Example 2

[0108] Under an anhydrous and oxygen-free inert environment, 2g of silicon suboxide and 0.1g of lithium metal flakes (the weight ratio of silicon suboxide powder to lithium metal is 20:1) were weighed and placed in a zirconia ball mill jar. After sealing, the jar was transferred to a nanoball mill for ball milling. The ball-to-material ratio was 20:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The milling was carried out at 50℃, a milling speed of 700 rpm, and a milling time of 24 hours. Then, 0.2g of artificial graphite was added and ball milling continued (the weight ratio of solid dispersant to lithium metal was 2:1). The milling was carried out at 50℃, a milling speed of 300 rpm, and a milling time of 1 hour. The powder was then removed and sealed in an anhydrous and oxygen-free inert environment for storage, yielding a silicon suboxide-based lithium supplementary powder, denoted as T-2.

[0109] Example 3

[0110] In an anhydrous and oxygen-free inert environment, 2g of silicon suboxide and 0.2g of lithium metal wire were weighed and placed in a zirconia ball mill jar (the weight ratio of silicon suboxide powder to lithium metal was 10:1). After sealing, the mixture was transferred to a nanoball mill for ball milling. The ball-to-material ratio was 20:1, and the zirconia balls had diameters of 5.5mm, 3.0mm, and 2.0mm in a ratio of 2:5:3. The milling was carried out at 50℃, with a milling speed of 900 rpm for 48 hours. Then, 0.02g of artificial graphite was added and ball milling continued (the weight ratio of solid dispersant to lithium metal was 0.1:1). The milling was carried out at 50℃, with a milling speed of 450 rpm for 1 hour. The powder was then removed and sealed in an anhydrous and oxygen-free environment for storage, yielding a silicon suboxide-based lithium supplement additive, denoted as T-3.

[0111] Example 4

[0112] The same preparation process as in Example 1 was used, except that:

[0113] Weigh 2g of silicon suboxide and 0.1g of lithium metal ingot (the weight ratio of silicon suboxide powder to lithium metal is 20:1) and place them in a zirconia ball mill jar;

[0114] Add 0.04g of natural graphite and continue ball milling (the weight ratio of solid dispersant to lithium metal is 0.4:1);

[0115] The remaining process is the same as in Example 1, and the resulting lithium supplementation additive product is denoted as T-4.

[0116] Example 5

[0117] The same preparation process as in Example 1 was used, except that:

[0118] The process conditions for ball milling silica powder and lithium metal were modified as follows: rotation speed of 600 r / min, homogenization time of 12 h, homogenization temperature of 80 ℃, and ball-to-material ratio of 30:1.

[0119] The process conditions during the ball milling process with natural graphite were modified as follows: rotation speed of 300 r / min, homogenization time of 4 h, homogenization temperature of 80 ℃, and ball-to-material ratio of 30:1. The resulting lithium supplementary additive product was denoted as T-5.

[0120] The test data of component content and structural parameters of the products obtained from the above embodiments and comparative examples are listed in Table 1 below.

[0121] Table 1

[0122]

[0123]

[0124] Test Example 1

[0125] This test example illustrates the electrochemical performance of the products obtained in the examples and comparative examples when used as lithium replenishment additives for the negative electrode of lithium-ion batteries. In the following battery manufacturing process, the conductive agent was carbon black (purchased from Tianjin Damao Chemical), and the binder was sodium carboxymethyl cellulose (purchased from Tianjin Damao Chemical).

[0126] (1) The additives prepared in the above examples and comparative examples are mixed with the graphite anode material at a weight ratio of 1:1 to form the anode material;

[0127] (2) Slurry preparation: Weigh the negative electrode material, conductive agent and binder in a ratio of 8:1:1, add solvent water to adjust the viscosity of the slurry, and stir for 3 hours;

[0128] (3) Coating: The slurry is coated onto the copper foil current collector using a doctor blade mold;

[0129] (4) Drying: Dry at 120℃ for 12 hours in a vacuum drying oven;

[0130] (5) Cutting: Cut into round battery negative electrode sheets with a diameter of 15mm, weigh them and place them in a drying oven;

[0131] (6) Assembly: In the glove box, CR2025 button cells are assembled using lithium sheets as the counter electrode.

[0132] The electrolyte was a 1M LiPF6 / EC:DMC (1:1, volume) mixture, and the diaphragm was a Celgard 2300 polypropylene microporous membrane.

[0133] The sealed batteries were left to stand for 24 hours, and then charge-discharge and cycle performance tests were conducted using the Land battery performance testing system. The test results are listed in Table 2.

[0134] Table 2

[0135]

[0136]

[0137] According to the data in Table 2:

[0138] Compared with the additive materials DT-1 to DT-3 prepared in Comparative Examples 1 to 3, the silicon suboxide-based lithium supplementation additives T-1 to T-5 prepared using the embodiments of this disclosure can effectively improve the first coulombic efficiency and cycle stability of lithium-ion batteries.

[0139] Furthermore, comparing Example 1 with Example 4, in Example 4, the weight ratio of silica powder to lithium metal in the lithium supplementation additive preparation process satisfies 10-50:1, and the weight ratio of solid dispersant to lithium metal satisfies 0.1-0.5:1. The additive obtained in Example 4 has a higher effect on improving the initial coulombic efficiency and cycle stability of lithium-ion batteries.

[0140] Comparing Example 1 and Example 5, it can be seen that the conditions of solid-phase homogenization reaction and dispersion homogenization reaction in the preparation process of Example 5 meet the preferred implementation method, and the additive obtained in Example 5 has a better effect on improving the first coulombic efficiency and cycle stability of lithium-ion batteries.

[0141] Test Example 2

[0142] This test example illustrates the performance of a lithium-ion battery prepared directly using a lithium-added additive as the negative electrode material (without adding graphite as the main material). The specific steps include:

[0143] (1) Slurry preparation: Weigh the negative electrode material (T-1 and T-2 prepared according to the examples), conductive agent and binder at a ratio of 8:1:1, add solvent water to adjust the viscosity of the slurry, and stir for 3 hours;

[0144] (2) Coating: The slurry is coated onto the copper foil current collector using a doctor blade mold;

[0145] (3) Drying: Dry in a vacuum drying oven at 120℃ for 12 hours;

[0146] (4) Cutting: Cut into round battery negative electrode sheets with a diameter of 15mm, weigh them and place them in a drying oven;

[0147] (5) Assembly: CR2025 button cell batteries are assembled in a glove box using lithium sheets as the counter electrode;

[0148] The electrolyte was a 1M LiPF6 / EC:DMC (1:1, vol) mixture, and the diaphragm was a Celgard 2300 polypropylene microporous membrane.

[0149] After sealing the battery and letting it stand for 24 hours, the Land battery performance testing system was used to conduct charge-discharge tests and cycle performance tests on the battery.

[0150] Figure 7 The electrochemical capacity-voltage test results of a lithium-ion battery assembled using the silicon suboxide-based powder lithium supplement additive material T-1 prepared in Example 1 are shown. At a current density of 0.2C, the initial charge specific capacity was 1200 mAh / g, and after 5 cycles, the capacity remained at 900 mAh / g, with subsequent cycling stability and almost no capacity decay. However, when using the silicon suboxide-based powder lithium supplement additive material alone as the negative electrode material, the aqueous solvent affected the performance test, preventing it from fully realizing its effect. Furthermore, comparing the performance of this test example with the lithium-ion batteries made using T-1 and graphite combinations listed in Table 2, Table 2 shows that using silicon suboxide-based lithium supplement additive T-1 as an additive in combination with the main negative electrode material (such as graphite negative electrode, silicon-carbon negative electrode, etc.) is more conducive to fully realizing its role in improving the initial coulombic efficiency and meeting the requirements of the aqueous slurry environment.

[0151] Figure 8 The electrochemical rate performance of batteries assembled using the silicon suboxide-based lithium supplement additive T-2 prepared in Example 2 as the negative electrode material is shown in the test results. The test current densities were 0.2C, 0.5C, 1.0C, 2.0C, 5.0C, 0.5C, and 0.2C. The silicon suboxide-based lithium supplement additive T-2 exhibited good rate performance; especially after a high rate cycle of 5.0C, when the test current density dropped to 0.5C and 0.2C, the specific capacity rapidly recovered and maintained good cycle stability.

[0152] Test Example 3

[0153] This test example illustrates the electrochemical performance of the product obtained in the examples when used as a lithium supplement additive in combination with a graphite host material.

[0154] The same battery assembly and testing methods as the test examples were used, except that the additives were mixed with the graphite anode material (main material) at weight ratios of 1:30 and 1:60 to serve as the anode material. The lithium supplementation additive used was T-1. The test results are listed in Table 3.

[0155] Table 3

[0156]

[0157] Comparing this test example with test example 1, it can be seen that the mixing weight ratio of additive T-1 to graphite anode material (main material) in test example 1 meets the requirement of "1 to 10:1". In the battery application of test example 1, in addition to having high initial coulombic efficiency and good cycle stability, the initial charge specific capacity and initial discharge specific capacity of test example 1 are much higher than those of test example 3, which meets the requirements of high energy density applications.

[0158] Test Comparison Example 1

[0159] A battery was assembled using silicon suboxide powder as the negative electrode material according to the process described in the test example, and its electrochemical performance was then tested.

[0160] Figure 9 To test the electrochemical capacity-voltage results of the lithium-ion battery assembled in Comparative Example 1, which directly used silicon suboxide powder as the negative electrode material, the current density was 0.2C. Figure 7 , Figure 8 ( Figure 8 (0.2C curve) and Figure 9 The comparison shows that, compared with Comparative Example 1 of this test, directly using the silicon suboxide-based lithium replenishment additive provided in this disclosure as the negative electrode material significantly improves the battery cycle stability and capacity retention. This indicates that the silicon suboxide-based lithium replenishment additive provided in this disclosure has good structural stability and can continuously replenish lithium during charge and discharge cycles, making up for the consumption and loss of lithium ions during battery cycles, thereby improving capacity cycle stability and retention.

[0161] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and all such simple modifications fall within the protection scope of this disclosure. For example...

[0162] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0163] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method for preparing a silicon suboxide-based lithium supplementary additive, characterized in that, The method includes the following steps: (1) Under an inert atmosphere, lithium metal and silicon suboxide powder are mixed and subjected to a solid-phase homogeneous reaction to obtain a reaction mixture; the weight ratio of silicon suboxide powder to lithium metal is (1~200):

1. (2) Under an inert atmosphere, the reaction mixture is mixed with a solid dispersant and then subjected to dispersion and homogenization treatment; Under an inert atmosphere, the material obtained in step (2) is sealed to obtain a silicon suboxide-based powder lithium supplementation additive; In step (1), the solid-phase homogenization reaction is carried out by ball milling; the conditions for the solid-phase homogenization reaction include: rotation speed of 200~1000 r / min, homogenization time of 2~48 h, homogenization temperature of 25~200 ℃, and ball-to-material ratio of (1~30):

1. In step (2), the dispersion and homogenization treatment is performed by ball milling; the conditions for the dispersion and homogenization treatment include: rotation speed of 100~450 r / min, time of 0.5~12 h, temperature of 25~200 ℃, and ball-to-material ratio of (1~30):

1.

2. The method according to claim 1, characterized in that, In step (1), the weight ratio of the silicon suboxide powder to the lithium metal is (10~50):

1.

3. The method according to claim 1, characterized in that, The median particle size of the silica powder is 1~20 μm; the average pore size is 1~50 nm; and the BET specific surface area is 0.5~100 m². 2 / g, total pore volume is 0.001~0.5cm³ 3 / g.

4. The method according to claim 3, characterized in that, The median particle size of the silica powder is 1~5 μm; the average pore size is 5~20 nm; and the BET specific surface area is 0.5~10 m². 2 / g, total pore volume is 0.001~0.1cm³ 3 / g.

5. The method according to claim 1, characterized in that, The chemical formula of the silica suboxide powder is SiO₂ x Where 0.5 ≤ x < 2; The lithium metal is selected from one or more of lithium ingots, lithium wires, lithium powder, or lithium sheets.

6. The method according to claim 1, characterized in that, In step (1), the conditions for solid-phase homogenization reaction include: rotation speed of 450~800 r / min, homogenization time of 10~24 h, homogenization temperature of 50~100 ℃, and ball-to-material ratio of (20~30):

1.

7. The method according to claim 1, characterized in that, In step (2), the solid dispersant is selected from one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon and soft carbon; The weight ratio of the solid dispersant to the lithium metal is (0.1~2):

1.

8. The method according to claim 7, characterized in that, The weight ratio of the solid dispersant to the lithium metal is (0.1~0.5):

1.

9. The method according to claim 1, characterized in that, In step (2), the conditions for dispersion and homogenization include: rotation speed of 100~300 r / min, homogenization time of 1~5 h, homogenization temperature of 50~100 ℃, and ball-to-material ratio of (20~30):

1.

10. The method according to claim 1, characterized in that, In steps (1) and (2), the inert atmosphere comprises one or more of nitrogen, helium, neon, argon, krypton and xenon; the water content of the inert atmosphere is less than 0.1% by weight and the oxygen content is less than 0.1% by weight.

11. A silicon suboxide-based lithium supplement additive prepared by the method according to any one of claims 1 to 10; wherein the silicon suboxide-based lithium supplement additive comprises silicon suboxide-based lithium supplement particles and a solid dispersant; wherein the silicon suboxide-based lithium supplement particles comprise a silicon suboxide matrix and a lithium-containing component, wherein the lithium-containing component is dispersed on the surface and / or within clusters of the silicon suboxide matrix; wherein the lithium-containing component comprises one or more of lithium silicate, lithium oxide, lithium, and lithium silicon alloy.

12. The silicon suboxide-based lithium supplementary additive according to claim 11, characterized in that, The weight ratio of silicon suboxide-based lithium supplementation particles to solid dispersant in the silicon suboxide-based lithium supplementation additive is (10~60):

1.

13. The silicon suboxide-based lithium supplementary additive according to claim 12, characterized in that, The weight ratio of silicon suboxide-based lithium supplementation particles to solid dispersant in the silicon suboxide-based lithium supplementation additive is (20~55):

1.

14. The silicon suboxide-based lithium supplementary additive according to claim 13, characterized in that, Based on the total weight of the silicon suboxide-based lithium supplement particles, the content of the lithium-containing component is 0.01~50% by weight.

15. The silicon suboxide-based lithium supplementary additive according to claim 14, characterized in that, Based on the total weight of the silicon suboxide-based lithium supplement particles, the content of the lithium-containing component is 0.9~20% by weight.

16. The silicon suboxide-based lithium supplementary additive according to claim 11, characterized in that, The silicon suboxide-based lithium supplement particles also contain elemental silicon, which is dispersed on the surface and / or within the clusters of the silicon suboxide matrix.

17. The silicon suboxide-based lithium supplementary additive according to claim 11, characterized in that, The silicon suboxide-based lithium supplement particles are diffusely dispersed in the solid dispersant.

18. The silicon suboxide-based lithium supplementary additive according to claim 11, characterized in that, The solid dispersant includes one or more of natural graphite, artificial graphite, mesophase carbon microspheres, hard carbon, and soft carbon.

19. The silicon suboxide-based lithium supplementary additive according to claim 11, characterized in that, The median particle size of the silicon suboxide-based lithium replenishing particles is 0.1~5μm; the average pore size is 1~50nm; and the BET specific surface area is 0.1~100m². 2 / g; total pore volume is 0.001~0.5cm³ 3 / g.

20. The silicon suboxide-based lithium supplementary additive according to claim 19, characterized in that, The median particle size of the silicon suboxide-based lithium replenishing particles is 0.1~1.5μm; the average pore size is 10~30nm; and the BET specific surface area is 1~35m². 2 / g; total pore volume is 0.05~0.2cm³. 3 / g.

21. A negative electrode composite material, characterized in that, The additive comprises the silicon suboxide-based lithium supplement as described in any one of claims 11 to 20.

22. The negative electrode composite material according to claim 21, characterized in that, The negative electrode composite material also includes a negative electrode main material; The negative electrode substrate material is selected from one or more of silicon suboxide negative electrode materials, graphite negative electrode materials, and silicon-carbon negative electrode materials.

23. The negative electrode composite material according to claim 22, characterized in that, The weight ratio of the negative electrode substrate material to the silicon suboxide-based lithium supplementation additive is (1~50):

1.

24. The negative electrode composite material according to claim 23, characterized in that, The weight ratio of the negative electrode substrate material to the silicon suboxide-based lithium supplementation additive is (1~10):

1.

25. The negative electrode composite material according to claim 22, characterized in that, The negative electrode composite material is prepared by a method including the following steps: The negative electrode substrate material is mixed with the silicon suboxide-based lithium supplementation additive.

26. A negative electrode, characterized in that, The negative electrode comprises the negative electrode composite material as described in any one of claims 21 to 25.

27. A lithium-ion battery, characterized in that, The lithium-ion battery includes the negative electrode as described in claim 26.

Citation Information

Patent Citations

  • Stabilized lithium metal powder for lithium-ion applications, composition and production process

    CN101790806A

  • Lithium ion battery cathode additive and preparation method thereof, lithium ion battery cathode piece and lithium ion battery

    CN103779572A

  • Preparation method of high-efficiency negative active material for lithium ion secondary battery

    CN109786670A

  • Preparation method of nano lithium silicide powder composite material as well as product and application thereof

    CN111129458A