Method for preparing 3D printing acellular dermal matrix skin scaffold bio-ink and using method thereof
The bio-ink for 3D printing decellularized dermal matrix skin scaffolds, prepared by combining gelatin methacrylic anhydride with decellularized dermal matrix, solves the problems of insufficient printability and bioactivity in existing technologies, achieving rapid prototyping and high biocompatibility, and is suitable for the precise construction of 3D bioprinted skin scaffolds.
Patent Information
- Application Number
- CN202311779722.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-22
AI Technical Summary
Existing bio-inks have problems such as poor printability, slow curing speed, low mechanical strength and insufficient bioactivity in 3D printed skin scaffolds, making it difficult to effectively promote wound healing.
A bio-ink for 3D printing decellularized dermal matrix skin scaffolds was prepared by combining gelatin methacrylic anhydride (GelMA) with decellularized dermal matrix. The ink achieves rapid prototyping and high biocompatibility through photopolymerization technology, while also regulating mechanical strength and bioactivity.
The prepared bio-ink has good printability, rapid curing ability and high bioactivity. It can accurately construct biomimetic three-dimensional structures, promote cell growth and tissue regeneration, and meet the needs of clinical skin substitutes.
Smart Images

Figure CN117752865B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of biological tissue engineering, specifically relating to a method for preparing bio-ink for 3D printing decellularized dermal matrix skin scaffolds. Background Technology
[0002] The incidence of diabetes mellitus (DM) in my country is increasing year by year, and diabetic foot ulcer (DFU) is one of its most significant complications. In the early stages of wound healing, inflammation, ischemia, infection, and oxidative stress can affect the wound, causing it to gradually become a chronic, difficult-to-heal wound. Without timely treatment, it can lead to amputation or even death. Currently, clinical treatment for diabetic wounds often employs a combination of novel moist dressings for segmented wound care, such as alginate dressings, film dressings, and hydrogel dressings. If the patient has severe skin loss, artificial skin grafting is necessary. Although these treatments have achieved some success, skin substitutes are expensive and their effectiveness is limited.
[0003] 3D bioprinting offers strong technical support for addressing the clinical shortage of skin substitutes. It utilizes bio-inks loaded with living cells, nucleic acids, and growth factors to precisely construct the desired skin tissue layer by layer, maintaining high cell viability. However, finding suitable bio-inks remains a major challenge in 3D bioprinting. An ideal bio-ink needs to simultaneously satisfy good printability (rapid curing ability), suitable mechanical support, excellent biocompatibility, and superior bioactivity. While some studies have utilized synthetic bio-inks such as gelatin and collagen to construct skin scaffolds in vitro, existing bio-inks still suffer from drawbacks in printability, including poor injection capability, slow curing speed, low mechanical strength, and uncontrollable degradation. Regarding bioactivity, existing bio-inks exhibit low bioactivity, failing to provide cells with a microenvironment similar to the in vivo ECM, resulting in insufficient nutrient supply, limited cell proliferation and tissue regeneration, and weak integration with newly formed wound tissue, thus failing to significantly promote wound healing. The lack of bio-inks possessing both good printability and bioactivity makes 3D printing of skin scaffolds a continued challenge. Decellularized matrix can provide cells with a microenvironment similar to the in vivo ECM, promoting cell proliferation and migration. However, its poor formability makes it difficult to print. Therefore, it needs to be combined with materials with better curing properties, such as gelatin methacrylic anhydride (GelMA), which has excellent biocompatibility and rapid photocuring ability. To solve the above problems, this invention prepares a bio-ink for 3D printing decellularized dermal matrix skin scaffolds. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing bio-ink for 3D printing decellularized dermal matrix skin scaffolds. This preparation method is simple and has low preparation cost. The prepared composite bio-ink contains extracellular matrix components, has excellent biocompatibility and bioactivity, and exhibits high three-dimensional cell culture activity with normal biological functions. When applied in the field of 3D bioprinting, it has good printability, ensuring high precision of the printed biomimetic three-dimensional structure, strong controllability of mechanical strength, and can accurately simulate the three-dimensional microenvironment of cell growth.
[0005] The technical solution adopted by this invention to achieve its objective is as follows:
[0006] A method for preparing a bio-ink for 3D printing decellularized dermal matrix skin scaffolds includes the following steps:
[0007] (A) Preparation of GelMA sponge: Gelatin was dissolved in D-PBS and stirred in a water bath at 50°C until the sample was completely dissolved. The pH of the solution was adjusted to 7.5-8.0 with 1 mol / L NaOH solution. Methacrylic anhydride was added at a constant rate. The solution was dialyzed in a water bath in the dark for 6 days and then freeze-dried for 48 hours to obtain GelMA sponge.
[0008] (B) Preparation of porcine decellularized dermal matrix: Fresh porcine skin tissue was pretreated, cut into small pieces, soaked in 0.25% trypsin for 6 hours, washed three times with deionized water, soaked in 70% ethanol for 10-12 hours, then soaked in 3% H2O2 for 15 minutes, washed once with deionized water, then soaked in a mixed solution of 1% Triton X-100 / 0.26% EDTA / 0.69% Tris for 20 hours, washed clean, and freeze-dried for 72 hours to prepare porcine decellularized dermal matrix;
[0009] (C) Preparation of acetone photoinitiator mixed solution: Dissolve the photoinitiator completely in acetone to prepare an acetone photoinitiator mixed solution;
[0010] (D) Preparation of composite bio-ink: Add the GelMA sponge from step (A) to PBS buffer and stir until fully dissolved at a suitable temperature. Slowly add the porcine decellularized dermal matrix from step (B) and the acetone photoinitiator mixture from step (C). The final concentration of GelMA is 0.125 g / ml and the concentration of porcine decellularized dermal matrix is 0.015-0.03 g / ml. After adjusting the pH and sterilizing, the product is ready.
[0011] As a preferred embodiment, in the above-mentioned method for preparing bio-ink for 3D printing decellularized dermal matrix skin scaffolds: methacrylic anhydride is added at a constant rate of 0.5 mL / min as described in step A.
[0012] As a preferred embodiment, in the above-mentioned method for preparing bio-ink for 3D printing decellularized dermal matrix skin scaffolds: the fresh pigskin pretreatment method in step (B) is to perform 5 freeze-thaw cycles at -80℃ and 37℃.
[0013] Preferably, in the above-mentioned method for preparing 3D printed decellularized dermal matrix skin scaffold bio-ink: the photoinitiator in step (C) is photoinitiator 184 and photoinitiator 819.
[0014] Preferably, in the above-mentioned method for preparing 3D printed decellularized dermal matrix skin scaffold bio-ink: the suitable temperature in step (D) is 50°C, and the pH is adjusted to 6.8-7.5.
[0015] As a preferred embodiment, in the above-mentioned method for preparing bio-ink for 3D printing decellularized dermal matrix skin scaffolds: step (D) is characterized in that the pH adjustment method is as follows: the composite bio-ink is placed on ice, and 1 mol / L NaOH solution is added dropwise while stirring rapidly.
[0016] The method of using the bio-ink for 3D printing decellularized dermal matrix skin scaffolds of the present invention is as follows:
[0017] The prepared bio-ink for 3D printing decellularized dermal matrix skin scaffolds was poured into the printing barrel. The printing barrel was fixed to the 3D printer nozzle, a printing needle with an inner diameter of 0.27mm was installed, the 3D printer parameters were set, and sterile printing was performed. The printed scaffold model was cured and cross-linked by irradiation with 365nm blue light, placed in a -40℃ freezer, and then soaked and cleaned to remove the photoinitiator. It was then vacuum freeze-dried and stored for later use.
[0018] The bio-ink for 3D printing decellularized dermal matrix skin scaffolds prepared by this invention exhibits excellent printability, high structural stability after cross-linking, and is made from widely available materials with high biosafety and biocompatibility. Furthermore, the preparation method is simple and low-cost. Compared with existing materials and technologies, this invention has the following advantages:
[0019] 1. The materials used in the decellularized dermal matrix skin scaffold bio-ink prepared by this invention are all derived from animals. The preparation conditions are mild and the preparation process is non-toxic and harmless. Moreover, the bio-ink retains the real extracellular matrix components, structure, properties and related physicochemical factors of tissue cells, and has good biodegradability, biocompatibility and bioactivity.
[0020] 2. The printed bio-ink can quickly cross-link and form within 30 seconds under 365nm blue light irradiation, exhibiting good printing performance and minimal damage to cells from blue light, thus meeting the requirements for cell-borne 3D bioprinting.
[0021] 3. By adjusting the proportion of decellularized extracellular matrix, the printability of the composite bio-ink is not affected. The mechanical strength and biological activity of the printed three-dimensional cell-loaded model can be effectively adjusted to meet the needs of model construction for tissues with different properties. Attached Figure Description
[0022] Figure 1 The bio-ink prepared according to the present invention.
[0023] Figure 2 This invention relates to a decellularized dermal matrix skin scaffold fabricated using the bio-ink prepared in this invention for 3D printing. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention are described clearly and completely below. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0025] Example 1
[0026] A method for preparing a bio-ink for 3D printing decellularized dermal matrix skin scaffolds includes the following steps:
[0027] (A) Preparation of GelMA sponge: Gelatin was dissolved in D-PBS and stirred in a water bath at 50°C until the sample was completely dissolved. The pH of the solution was adjusted to 7.5-8.0 with 1 mol / L NaOH solution. Methacrylic anhydride was added at a constant rate. The solution was dialyzed in a water bath in the dark for 6 days and then freeze-dried for 48 hours to obtain GelMA sponge.
[0028] (B) Preparation of porcine decellularized dermal matrix: Fresh porcine skin tissue was pretreated, cut into small pieces, soaked in 0.25% trypsin for 6 hours, washed three times with deionized water, soaked in 70% ethanol for 10-12 hours, then soaked in 3% H2O2 for 15 minutes, washed once with deionized water, then soaked in a mixed solution of 1% Triton X-100 / 0.26% EDTA / 0.69% Tris for 20 hours, washed clean, and freeze-dried for 72 hours to prepare porcine decellularized dermal matrix;
[0029] (C) Preparation of acetone photoinitiator mixed solution: Dissolve the photoinitiator completely in acetone to prepare an acetone photoinitiator mixed solution;
[0030] (D) Preparation of composite bio-ink: Add the GelMA sponge from step (A) to PBS buffer and stir until fully dissolved at a suitable temperature. Slowly add the porcine decellularized dermal matrix from step (B) and the acetone photoinitiator mixture from step (C) until the final concentration of GelMA is 0.125 g / ml and the concentration of porcine decellularized dermal matrix is 0.015 g / ml. After adjusting the pH and sterilizing, the product is ready.
[0031] Example 2
[0032] A method for preparing a bio-ink for 3D printing decellularized dermal matrix skin scaffolds includes the following steps:
[0033] (A) Preparation of GelMA sponge: Gelatin was dissolved in D-PBS and stirred in a water bath at 50°C until the sample was completely dissolved. The pH of the solution was adjusted to 7.5-8.0 with 1 mol / L NaOH solution. Methacrylic anhydride was added at a constant rate. The solution was dialyzed in a water bath in the dark for 6 days and then freeze-dried for 48 hours to obtain GelMA sponge.
[0034] (B) Preparation of porcine decellularized dermal matrix: Fresh porcine skin tissue was pretreated, cut into small pieces, soaked in 0.25% trypsin for 6 hours, washed three times with deionized water, soaked in 70% ethanol for 10-12 hours, then soaked in 3% H2O2 for 15 minutes, washed once with deionized water, then soaked in a mixed solution of 1% Triton X-100 / 0.26% EDTA / 0.69% Tris for 20 hours, washed clean, and freeze-dried for 72 hours to prepare porcine decellularized dermal matrix;
[0035] (C) Preparation of acetone photoinitiator mixed solution: Dissolve the photoinitiator completely in acetone to prepare an acetone photoinitiator mixed solution;
[0036] (D) Preparation of composite bio-ink: Add the GelMA sponge from step (A) to PBS buffer and stir until fully dissolved at a suitable temperature. Slowly add the porcine decellularized dermal matrix from step (B) and the acetone photoinitiator mixture from step (C) until the final concentration of GelMA is 0.125 g / ml and the concentration of porcine decellularized dermal matrix is 0.03 g / ml. After adjusting the pH and sterilizing, the ink is ready.
[0037] Example 3
[0038] A method for preparing a bio-ink for 3D printing decellularized dermal matrix skin scaffolds includes the following steps:
[0039] (A) Preparation of GelMA sponge: Gelatin was dissolved in D-PBS and stirred in a water bath at 50°C until the sample was completely dissolved. The pH of the solution was adjusted to 7.5-8.0 with 1 mol / L NaOH solution. Methacrylic anhydride was added at a constant rate. The solution was dialyzed in a water bath in the dark for 6 days and then freeze-dried for 48 hours to obtain GelMA sponge.
[0040] (B) Preparation of porcine decellularized dermal matrix: Fresh porcine skin tissue was pretreated, cut into small pieces, soaked in 0.25% trypsin for 6 hours, washed three times with deionized water, soaked in 70% ethanol for 10-12 hours, then soaked in 3% H2O2 for 15 minutes, washed once with deionized water, then soaked in a mixed solution of 1% Triton X-100 / 0.26% EDTA / 0.69% Tris for 20 hours, washed clean, and freeze-dried for 72 hours to prepare porcine decellularized dermal matrix;
[0041] (C) Preparation of acetone photoinitiator mixed solution: Dissolve the photoinitiator completely in acetone to prepare an acetone photoinitiator mixed solution;
[0042] (D) Preparation of composite bio-ink: Add the GelMA sponge from step (A) to PBS buffer and stir until fully dissolved at a suitable temperature. Slowly add the porcine decellularized dermal matrix from step (B) and the acetone photoinitiator mixture from step (C) until the final concentration of GelMA is 0.125 g / ml and the concentration of porcine decellularized dermal matrix is 0.02 g / ml. After adjusting the pH and sterilizing, the product is ready.
[0043] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a bio-ink for 3D printing decellularized dermal matrix skin scaffolds, characterized in that... Includes the following steps: (A) Preparation of GelMA sponge: Gelatin was dissolved in D-PBS and stirred in a water bath at 50°C until the sample was completely dissolved. The pH of the solution was adjusted to 7.5-8.0 with 1 mol / L NaOH solution. Methacrylic anhydride was added at a constant rate. The solution was dialyzed in a water bath in the dark for 6 days and then freeze-dried for 48 hours to obtain GelMA sponge. (B) Preparation of porcine decellularized dermal matrix: Fresh porcine skin tissue was pretreated, cut into small pieces, soaked in 0.25% trypsin for 6 hours, washed three times with deionized water, soaked in 70% ethanol for 10-12 hours, soaked in 3% H2O2 for 15 minutes, washed once with deionized water, then soaked in a mixed solution of 1% Triton X-100 / 0.26% EDTA / 0.69% Tris for 20 hours, washed clean, and freeze-dried for 72 hours to prepare porcine decellularized dermal matrix; (C) Preparation of acetone photoinitiator mixed solution: Dissolve the photoinitiator completely in acetone to prepare an acetone photoinitiator mixed solution; (D) Preparation of composite bio-ink: Add the GelMA sponge from step (A) to PBS buffer and stir until fully dissolved at a suitable temperature. Slowly add the porcine decellularized dermal matrix from step (B) and the acetone photoinitiator mixture from step (C) until the final concentration of GelMA is 0.125 g / ml and the concentration of porcine decellularized dermal matrix is 0.015-0.03 g / ml. After adjusting the pH and sterilizing, the product is ready. The fresh pigskin pretreatment method described in step (B) involves five freeze-thaw cycles at -80°C and 37°C. The photoinitiators mentioned in step (C) are photoinitiator 184 and photoinitiator 819.
2. The method for preparing the 3D-printed decellularized dermal matrix skin scaffold bio-ink according to claim 1, characterized in that: The constant rate described in step (A) is 0.5 mL / min.
3. The method for preparing the 3D-printed decellularized dermal matrix skin scaffold bio-ink according to claim 1, characterized in that: The suitable temperature described in step (D) is 50°C, and the pH is adjusted to 6.8-7.
5.
4. The method for preparing the 3D-printed decellularized dermal matrix skin scaffold bio-ink according to claim 1, characterized in that: The pH adjustment method is as follows: place the composite bio-ink on ice and add 1 mol / L NaOH solution dropwise while stirring rapidly.
5. The method of using the bio-ink for 3D printing decellularized dermal matrix skin scaffolds according to claim 1, characterized in that... Includes the following steps: Pour the prepared bio-ink for 3D printing decellularized dermal matrix skin scaffold into the printing cylinder, fix the printing cylinder to the 3D printer nozzle, install the printing needle with an inner diameter of 0.27mm, set the 3D printer parameters, and perform sterile printing. The printed scaffold model was cured and cross-linked by irradiation with 365nm blue light, then frozen in a -40℃ freezer. After removing the photoinitiator by soaking and cleaning, it was vacuum freeze-dried and stored for later use.