A method for preparing a transition metal-doped RuO2 catalyst
By preparing transition metal-doped RuO₂ catalysts on carbon nanotubes, the stability problem of RuO₂ catalysts under acidic conditions was solved, achieving high efficiency and stability of acidic OER and simplifying the synthesis process.
Patent Information
- Application Number
- CN202410142566.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-02-01
AI Technical Summary
Existing RuO₂ catalysts exhibit poor stability under acidic conditions, and current synthesis methods are complex and difficult to effectively combine with carbon nanotubes, thus affecting catalytic activity and stability.
Using carbon nanotubes as a support, a transition metal-doped RuO₂ catalyst was prepared through a simple impregnation and annealing process. This process restricted the particle size, increased the active area, and provided a faster electron transport rate through the carbon nanotubes.
The oxygen evolution reaction overpotential in 0.5 M H₂SO₄ is lower than that of commercial RuO₂, and the catalyst exhibits excellent stability and activity under acidic conditions, with significantly improved catalytic performance.
Smart Images

Figure CN117753411B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysis, and more particularly to a method for preparing a transition metal-doped RuO2 catalyst. Background Technology
[0002] Electrolysis of water is a highly efficient, environmentally friendly, and renewable hydrogen production technology. Currently, there are four main types of water electrolysis hydrogen production technologies: alkaline electrolysis (ALK), proton exchange membrane electrolysis (PEM), solid oxide electrolysis (SOEC), and anion exchange membrane electrolysis (AEM). Among them, proton exchange membrane electrolysis (PEMWE) has attracted significant research interest due to its advantages such as low ohmic loss, high current density, ultra-high gas purity, and excellent voltage efficiency. PEMWE technology mainly involves two half-reactions: the oxygen evolution reaction (OER) occurring at the anode and the hydrogen evolution reaction (HER) occurring at the cathode. The anode OER involves a complex four-proton coupled electron transfer process, and the high reaction energy barrier limits the overall water splitting efficiency. Furthermore, because PEMWE is a strong acid and strong oxidizing environment, it leads to irreversible dissolution and corrosion of metal catalysts. Therefore, developing OER catalysts with high catalytic activity, corrosion resistance, and high stability is crucial.
[0003] Currently, catalysts used in acidic OER reactions mainly rely on noble metal materials such as IrO2 and RuO2. Compared to IrO2, RuO2 has poorer corrosion resistance in strong acids, but it is more expensive due to the greater scarcity of Ir. Furthermore, most studies indicate that during the OER reaction, the reaction intermediate (O... * OH * and OOH * Ru exhibits moderate binding strength at Ru sites. Therefore, RuO2 catalysts possess relatively high activity for oxygen evolution. However, it is worth noting that excessive oxidation of Ru metal under acidic conditions leads to the formation of oxides rich in high-valence Ru, resulting in rapid catalyst deactivation. Therefore, there is an urgent need to find an effective way to enhance the stability of RuO2 under acidic conditions.
[0004] Current methods for modifying RuO2 mainly rely on elemental doping, morphology control, and the construction of heterostructures. Elemental doping and heterostructure construction can significantly reduce catalyst costs without sacrificing catalytic activity, thus attracting widespread attention. However, most existing synthesis methods are quite complex, thus limiting their effectiveness. Here, we propose a simpler synthesis method that yields transition metal-doped RuO2 uniformly dispersed on carbon nanotubes (CNTs), achieving superior acidic OER activity and stability.
[0005] Currently, the commonly used methods for synthesizing transition metal-doped RuO2 catalysts mainly rely on two approaches: the sol-gel method and the solid-state sintering method. The sol-gel method yields a relatively uniform elemental distribution in the transition metal-doped RuO2 solid solution, achieving homogeneous doping at the molecular level, but the reaction cycle is relatively long. The solid-state sintering method can produce catalysts with better crystallinity, but the size is relatively large, resulting in less exposure of the active surface. Furthermore, neither of these methods can directly bond well with carbon nanotubes, requiring further grinding or annealing. Summary of the Invention
[0006] To improve the time and efficiency of catalyst synthesis, this invention provides a relatively simple synthesis method for obtaining transition metal-doped RuO2 uniformly loaded onto CNTs. In this application, the introduction of carbon nanotubes effectively limits the particle size of the transition metal-doped RuO2 catalyst, increasing the active surface area. Furthermore, carbon nanotubes can provide a faster electron transport rate, further improving the catalytic performance of the catalyst.
[0007] This invention employs the following technical solution: a method for preparing a transition metal-doped RuO2 catalyst, wherein the transition metal-doped RuO2 catalyst is uniformly supported on CNTs, comprising the following steps:
[0008] (1) Disperse the carrier CNTs in ethanol by ultrasonication for more than one hour;
[0009] (2) Add Ru salt and transition metal salt, and treat under ultrasonic conditions for more than 40 minutes to allow the metal ligands to react fully;
[0010] (3) After evaporating the solvent ethanol, grind the sample thoroughly in a mortar.
[0011] (4) Transfer to a crucible and anneal in air atmosphere at a temperature of 250-400℃ and a heating rate of 5℃ / min to obtain the transition metal-doped RuO2 catalyst supported on CNTs.
[0012] Further, the Ru salt is ruthenium acetylacetonate or ruthenium chloride. The transition metal salt is an acetylacetonate or a chloride. Since metal acetylacetonate / chloride salts are soluble in most organic solvents, such as alcohols, benzene, and hexane, they can be well dispersed and reacted in ethanol. Furthermore, CNTs have a certain degree of hydrophobicity but can still disperse well in ethanol. Because the nucleation sites of ruthenium oxide are random, well-dispersed carbon nanotubes largely limit the nucleation and growth of ruthenium oxide, reducing the grain size and preventing large-area agglomeration of ruthenium oxide grains, thereby increasing the exposure probability of the catalyst's active surface and improving the catalyst's catalytic activity.
[0013] Preferably, the transition metal is Fe.、 Co 、 Zn or Mn.
[0014] Furthermore, the ratio of Ru salt to transition metal salt, expressed as a molar ratio of Ru to transition metal, is 1:0.5 to 1:2.
[0015] Furthermore, the method for evaporating the solvent ethanol is as follows: first, evaporate the solvent ethanol using a rotary evaporator at a temperature of 45°C, and then place it in a 60°C oven overnight.
[0016] Furthermore, the CNTs undergo pretreatment, specifically: the CNTs are placed in a vacuum filtration apparatus and concentrated hydrochloric acid is added to the apparatus for cleaning; after washing several times, deionized water is added for further cleaning until the waste liquid is neutral; then the washed CNTs are placed in a 60°C oven to dry them completely; finally, the dried CNTs are thoroughly ground for later use.
[0017] The beneficial effects of this invention are as follows: the overpotential of the catalyst obtained in this application for the oxygen evolution reaction in 0.5M H2SO4 is all above 280mV, with the lowest reaching 210mV, which is significantly lower than the 300mV of commercial RuO2. Compared with the sol-gel method and solid-state sintering method, the preparation method of this application, which uses a simple impregnation method combined with subsequent annealing, can relatively easily obtain a RuO2 catalyst with relatively uniform elemental doping and transition metal doping, and the catalyst is uniformly distributed on the CNT support with uniform nanoparticle size. Attached Figure Description
[0018] Figure 1 XRD data of the catalysts prepared in Examples 1 to 6.
[0019] Figure 2 Linear sweep voltammetric curves of the catalysts prepared in Examples 1 to 6 in 0.5 M H2SO4.
[0020] Figure 3 SEM image of the catalyst in Example 1.
[0021] Figure 4 SEM image of the catalyst in Example 2.
[0022] Figure 5 SEM image of the catalyst in Example 3.
[0023] Figure 6 SEM image of the catalyst in Example 4.
[0024] Figure 7 SEM image of the catalyst in Example 5.
[0025] Figure 8SEM image of the catalyst in Example 6.
[0026] Figure 9 TEM image of the catalyst in Comparative Example 1.
[0027] Figure 10 TEM image of the catalyst in Comparative Example 2.
[0028] Figure 11 TEM image of the catalyst in Comparative Example 3.
[0029] Figure 12 Linear sweep voltammetric curves of the catalysts prepared in Example 1 and Comparative Examples 1 to 3 in 0.5 M H2SO4. Detailed Implementation
[0030] In the following embodiments, the carrier CNTs used are commercially available CNTs. However, since commercial CNTs may contain impurities, they need to be pretreated. The specific procedure is as follows: An appropriate amount of CNTs is placed in a vacuum filtration apparatus, and concentrated hydrochloric acid is added to the apparatus for washing. After washing several times, deionized water is added for further washing until the waste liquid is neutral. Then, the washed CNTs are placed in a 60°C oven to dry completely. Finally, the dried CNTs are thoroughly ground for later use.
[0031] Case Study 1:
[0032] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0033] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 35.317 mg (0.1 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0034] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0035] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0036] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The FeRuO2 catalyst supported on CNTs can then be obtained.
[0037] Case Study 2:
[0038] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0039] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetonate and 25.715 mg (0.1 mmol) of cobalt acetylacetonate respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0040] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0041] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0042] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300°C and a heating rate of 5°C / min. The CoRuO2 catalyst supported on CNTs can then be obtained.
[0043] Case Study 3:
[0044] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0045] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 25.69 mg (0.1 mmol) of nickel acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0046] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0047] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0048] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The NiRuO2 catalyst supported on CNTs can then be obtained.
[0049] Case Study 4:
[0050] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0051] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 26.176 mg (0.1 mmol) of copper acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0052] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0053] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0054] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The CuRuO2 catalyst supported on CNTs can then be obtained.
[0055] Case Study 5:
[0056] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0057] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetonate and 26.361 mg (0.1 mmol) of zinc acetylacetonate respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0058] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0059] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0060] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The ZnRuO2 catalyst supported on CNTs is then obtained.
[0061] Case Study 6:
[0062] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0063] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 35.227 mg (0.1 mmol) of manganese acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0064] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0065] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0066] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The MnRuO2 catalyst supported on CNTs can then be obtained.
[0067] Case Study 7:
[0068] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0069] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 17.659 mg (0.05 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0070] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0071] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0072] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The FeRu2O2 catalyst supported on CNTs is then obtained.
[0073] Case Study 8:
[0074] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0075] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 70.634 mg (0.2 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0076] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0077] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0078] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 300℃ and a heating rate of 5℃ / min. The Fe2RuO2 catalyst supported on CNTs can then be obtained.
[0079] Case Study 9:
[0080] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0081] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 35.317 mg (0.1 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0082] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0083] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0084] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 250°C and a heating rate of 5°C / min. The Fe2RuO2 catalyst supported on CNTs is then obtained.
[0085] Case Study 10:
[0086] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0087] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 35.317 mg (0.1 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0088] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0089] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0090] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 350°C and a heating rate of 5°C / min. The FeRuO2 catalyst supported on CNTs is then obtained.
[0091] Case Study 11:
[0092] (1) Weigh 50 mg of pretreated carrier CNTs into a flask, then add 20 ml of ethanol to the flask and sonicate in an ultrasonic machine for one hour to ensure that the carriers are fully and evenly dispersed.
[0093] (2) Weigh 39.839 mg (0.1 mmol) of ruthenium acetylacetone and 35.317 mg (0.1 mmol) of iron acetylacetone respectively, and add them to the flask after sonication in step (1) in sequence. Continue sonication for 40 minutes to allow the metal ligands to react fully.
[0094] (3) After evaporating the solvent ethanol from the flask in step (2) using a rotary evaporator at a temperature of 45°C, place it in a regular 60°C oven overnight to allow the residual solvent to dry completely.
[0095] (4) After scraping the sample from the flask in step (3) with a spatula, grind it thoroughly in a mortar.
[0096] (5) Finally, the ground sample is placed in a crucible and annealed in an air atmosphere in a muffle furnace at a temperature of 400℃ and a heating rate of 5℃ / min. The FeRuO2 catalyst supported on CNTs can then be obtained.
[0097] Comparative Example 1
[0098] This example is the same as Case 1, except that in step 1, the CNTs are dispersed in ethanol and ultrasonically dispersed for 0.5 hours.
[0099] Comparative Example 2
[0100] This example is similar to Case 1, except that in step 1, the metal salt was not evenly dispersed by ultrasound after being added to ethanol.
[0101] Comparative Example 3
[0102] This example is similar to Case 1, except that in step 1, the CNTs are dispersed in ethanol and ultrasonically dispersed for 0.5 hours, and the ultrasonic dispersion of the metal salt is uneven after the metal salt is added to the ethanol.
[0103] The products from Examples 1 to 6 were tested using linear sweep voltammetry (LSV) in 0.5 M H₂SO₄, and the results are as follows: Figure 2 As shown in the figure, all catalysts exhibited good catalytic activity at 10 mA / cm². -2 The overpotentials at the current density were all lower than those of commercial RuO2, with the best-performing catalyst having an overpotential of only around 200 mV. This confirms that transition metals enhance the acidic OER activity of RuO2 and also demonstrates the advantages of our synthesis method.
[0104] XRD data for Implementation Cases 1 through 6 are shown below. Figure 1 As shown in the figure, the catalyst exhibits an overall RuO2 structure, and no characteristic peaks of doped metals or their oxides are observed. This indicates that the transition metal has been effectively incorporated into the RuO2 structure, achieving the expected results. SEM data for Implementation Cases 1 through 6 are shown below. Figures 3-8 As can be seen from the figure, small-sized oxide nanoparticles are uniformly loaded on the CNT support. Additionally, Fe... 、 Co 、 Zn 、 Mn-doped RuO2 nanoparticles are smaller in size than Cu-doped RuO2 nanoparticles, which may be due to Fe... 、 Co 、 Zn 、 The property of Mn combining with RuO2 brings about this, from Figure 2 As can also be seen in the LSV curve, Fe 、 Co 、 Zn 、 Mn-doped catalysts exhibit better catalytic performance than Cu-doped RuO2 nanoparticles.
[0105] TEM data for Comparative Examples 1 to 3 are shown in Figures 9-11As can be seen from the figure, unevenly dispersed CNTs cannot effectively exert their confinement effect, and the ruthenium oxide nanoparticles are relatively large. The products of Example 1 and Comparative Examples 1-3 were subjected to linear sweep voltammetry (LSV) testing in 0.5M H₂SO₄, and the results are as follows... Figure 12 As shown, large catalyst particles significantly affect catalytic performance.
Claims
1. A method for preparing a transition metal-doped RuO2 catalyst, characterized in that, The transition metal-doped RuO2 catalyst is uniformly loaded onto CNTs, comprising the following steps: (1) Disperse the carrier CNTs in ethanol by ultrasonication for more than one hour to ensure uniform dispersion of CNTs; (2) Add Ru salt and transition metal salt, and treat under ultrasonic conditions for more than 40 minutes to allow the metal ligands to react fully; (3) After evaporating the solvent ethanol, grind the sample thoroughly in a mortar; (4) Transfer to a crucible and anneal in air atmosphere at a temperature of 250-400℃ and a heating rate of 5℃ / min to obtain the transition metal doped RuO2 catalyst supported on CNTs.
2. The method according to claim 1, characterized in that, The Ru salt is ruthenium acetylacetonate or ruthenium chloride.
3. The method according to claim 1, characterized in that, The transition metal salt is an acetylacetone salt or a chloride salt; the transition metal is Fe, Co, Zn or Mn.
4. The method according to claim 1, characterized in that, Ru salts and transition metal salts are in a molar ratio of Ru to transition metal of 1:0.5 to 1:
2.
5. The method according to claim 1, characterized in that, The method for evaporating the solvent ethanol is as follows: first, evaporate the solvent ethanol using a rotary evaporator at a temperature of 45°C, and then place it in a 60°C oven overnight.
6. The method according to claim 1, characterized in that, The CNTs first undergo pretreatment, specifically: the CNTs are placed in a vacuum filtration apparatus and concentrated hydrochloric acid is added to the apparatus for washing; after washing several times, deionized water is added for washing again until the waste liquid is neutral; then the washed CNTs are placed in a 60°C oven to dry them completely; finally, the dried CNTs are thoroughly ground for later use.
Citation Information
Patent Citations
Metallic oxide / N-doped carbon nano tube as well as preparation method and application thereof
CN103170324A
Novel high-dispersion transition metal doped RuO2 / C composite material and preparation method thereof
CN111545218A
Mn-Co3O4-coated CNTs-O electrocatalyst as well as preparation method and application thereof