A method of floating lepidolite

By selectively suppressing feldspar using ferric ions in the flotation of lepidolite, the process is simplified to one coarse, one fine, and one scavenging step, solving the problems of high difficulty and cost in separating lepidolite from feldspar, and achieving efficient and low-cost lepidolite recovery.

CN117753563BActive Publication Date: 2026-11-24ZHENGZHOU UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410106465.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2026-11-24
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

Existing lepidolite flotation processes suffer from problems such as high separation difficulty, high cost, high energy consumption, low resource recovery rate, and environmental pollution. In particular, the similar surface chemical structure and floatability of feldspar and lepidolite cause great separation difficulties.

Method used

Using ferric ions as a selective inhibitor, feldspar is selectively suppressed during the flotation process, simplifying the process to one roughing, one cleaning, and one scavenging step. By altering the surface electrical properties of gangue minerals through electrostatic adsorption, efficient recovery of lepidolite is achieved.

Benefits of technology

It improves the recovery rate of lepidolite and the grade of concentrate, shortens the sorting process, reduces energy consumption and production costs, and reduces tailings volume, which is in line with the concept of green mining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117753563B_ABST
    Figure CN117753563B_ABST
Patent Text Reader

Abstract

The application discloses a method for floating lepidolite, which comprises the following steps: S1, adjusting the pH of the roughing concentrate slurry to 2-10, adding Fe 3+ and a collector dodecylamine in sequence, and then performing air blowing and bubble scraping to obtain a roughing foam product and a scavenging feed ore respectively; S2, adding Fe 3+ and the collector dodecylamine in the scavenging feed ore obtained in the step S1, and performing air blowing and bubble scraping to obtain a scavenging foam product and a tailing; S3, adjusting the pH of the roughing foam product obtained in the step S1 and the scavenging foam product obtained in the step S2 to 2-10, adding Fe 3+ , and then performing air blowing and bubble scraping to obtain a lepidolite concentrate. In the method, the trivalent iron ion can selectively inhibit feldspar, such as potassium feldspar, sodium feldspar and other feldspar aluminosilicate minerals, in the lepidolite ore in the process of flotation, and can effectively improve the grade recovery rate of the lepidolite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to mineral flotation processes, and more specifically, to a flotation method for lepidolite. Background Technology

[0002] Currently, lithium extraction in my country primarily relies on pegmatite. Major exploited pegmatite-type lithium resources in my country include spodumene from Koktokay in Xinjiang and northwestern Sichuan, lepidolite from the Yichun tantalum-niobium mine in Jiangxi, and lepidolite from Tongcheng in Hubei. Among these, the Yichun tantalum-niobium mine in Jiangxi possesses the world's largest associated lepidolite deposit. Lepidolite reserves are abundant, making it a crucial resource for lithium extraction. Currently, flotation is widely considered the most economical and effective method for lithium extraction. However, lepidolite is often associated with various gangue minerals, primarily feldspar. Due to their similar surface chemical structure and floatability to lepidolite, separation becomes extremely difficult.

[0003] In the industrial production of lithium extraction from lepidolite, a flotation process of one roughing stage, four cleaning stages, and one scavenging stage is typically used to achieve good production indicators. However, a multi-stage cleaning process means that more flotation machines are needed, increasing production costs and requiring a larger production workshop. In addition, the multi-stage flotation process also increases energy consumption, while also resulting in greater product loss and a decrease in resource recovery rate.

[0004] Meanwhile, traditional flotation processes typically use water glass, sodium hexametaphosphate, oxalic acid, carboxymethyl cellulose, etc. as depressants, which have problems such as large depressant usage, low resource recovery rate, difficulty in removal, and easy environmental impact. Therefore, a cleaner and more economical method is needed to achieve efficient separation of lepidolite. Summary of the Invention

[0005] To address the issue of the lengthy flotation process for lepidolite, this invention provides a flotation method for lepidolite. By employing trivalent iron ions to efficiently and selectively suppress feldspar, the flotation process is simplified, thereby enabling efficient flotation and recovery of lepidolite.

[0006] To achieve the above objectives, the present invention provides a flotation method for lithium mica, the flotation method comprising the following steps: S1. Adjust the pH of the roughing concentrate slurry to 2-10, and add Fe sequentially. 3+ The mixture was then subjected to aeration and foaming with dodecylamine as a collector, and the roughing froth product and scavenging feed were obtained, respectively. S2. Add Fe to the scavenged feed obtained in step S1. 3+ The product and tailings were obtained by aeration and foaming with the collector dodecylamine and the aeration and foaming process. S3. Adjust the pH of the coarse foam product obtained in step S1 and the scavenging foam product obtained in step S2 to 2-10, and add Fe.3+ Then, aeration and foaming were performed to obtain lepidolite concentrate.

[0007] This invention utilizes the ultra-low negative potential of minerals such as quartz and feldspar, and the strong affinity of iron ions for non-metallic oxides, by adding Fe during the roughing process. 3+ With a pulp pH of 2-10, and without introducing organic inhibitors, a short process of one rougher, one cleaner, and one scavenger replaced the conventional long process of one rougher, four cleaners, and one scavenger, achieving selective modification of lepidolite and gangue, and Fe... 3+ By selectively acting on gangue minerals through electrostatic adsorption, this invention alters their surface charge, inhibits flotation, significantly improves concentrate grade and recovery rate, shortens the separation process, and reduces tailings production. This invention overcomes the problems of insufficient selective inhibition capacity, large tailings pollution, and organic pollutants in wastewater associated with traditional flotation depressants. It significantly improves processing efficiency, shortens the beneficiation process, and reduces upfront infrastructure investment, resulting in not only significant economic benefits but also aligning with the concept of green mining.

[0008] Preferably, in step S1, the method for obtaining the concentrate slurry is as follows: the raw ore is wet-milled and then deslimed to obtain the rough concentrate slurry.

[0009] The raw ore has a Li2O grade of 0.8% to 0.9%, and the desliming amount is 5% to 8%.

[0010] The grinding concentration is 25-45%, preferably 30%-40%.

[0011] Fe 3+ It is derived from soluble iron salts, such as ferric chloride hexahydrate, ferric nitrate, and ferric sulfate. When applicable, the soluble iron salt is prepared into a solution with a mass concentration of 1% to 3%.

[0012] In step S1, Fe 3+ The reagent addition amount is 300-600 g / t. In step S2, Fe... 3+ The reagent addition amount is 150-300 g / t. In step S3, Fe... 3+ The reagent addition amount is 75-150g / t.

[0013] In steps S1 to S2, the collector is a mixture of dodecylamine and hydrochloric acid / acetic acid.

[0014] Specifically, the mass ratio of the components of Hohhot is: 1% dodecylamine, 1%~3% hydrochloric acid / acetic acid, and 96%~98% water. The preparation method is as follows: dodecylamine is placed in a beaker, and hydrochloric acid / acetic acid is added to dissolve it, generating hydrochloride / acetic acid salts. After the reaction is complete, water is added to dilute it for later use, thus preparing a collector.

[0015] The amount of dodecylamine added in step S1 is 160-240 g / t, and the amount of dodecylamine added in step S2 is 80-120 g / t.

[0016] In steps S1 and S3, the pH of the slurry is adjusted to 4-8, respectively.

[0017] During the flotation process, the temperature of the pulp is 5~50℃.

[0018] Through the above technical solution, the present invention achieves the following beneficial effects: 1. This invention utilizes ferric ions during the flotation process to selectively suppress feldspar, such as potassium feldspar and sodium feldspar, and other feldspar aluminosilicate minerals in lepidolite ore, thereby effectively improving the grade recovery rate of lepidolite.

[0019] 2. The present invention uses a small amount of metal ion inhibitor, which simplifies the flotation process, significantly reduces energy consumption and resource loss, and at the same time reduces the difficulty of treating mineral processing wastewater, making it environmentally friendly. Attached Figure Description

[0020] Figure 1 is a flowchart of the experiment of flotation of pure lithium mica minerals with trivalent iron ion inhibitor in Example 1; Figure 2 is a flowchart of the actual experiment of flotation of lithium mica ore using trivalent iron ion inhibitor in Example 2. Detailed Implementation

[0021] The specific embodiments of the present invention will be described in detail below with reference to examples. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0022] In the following examples, the iron ion solution is prepared as follows: ferric chloride hexahydrate reagent is dissolved in deionized water to prepare a solution with a mass concentration of 1%.

[0023] The collector is prepared as follows: Weigh dodecylamine, hydrochloric acid and water in a mass ratio of 1:1:98. Place the dodecylamine in a beaker, add hydrochloric acid to dissolve it, and generate hydrochloride. After the reaction is complete, dilute with water for later use.

[0024] Example 1 This example uses pure lepidolite ore from Yunnan (lepidolite purity exceeds 95%), and its main components are as follows: Table 1. Chemical elemental analysis results (%) of lepidolite Element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[K2O]]> <![CDATA[Li2O]]> <![CDATA[Rb2O]]> MnO <![CDATA[Na2O]]> <![CDATA[Cs2O]]> content 52.62 21.13 13.02 5.50 2.02 1.13 0.36 0.23 Table 2. Chemical elemental analysis results of feldspar (%) Element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Na2O]]> CaO <![CDATA[K2O]]> content 68.69 18.16 12.33 0.42 0.11 use Figure 1The flotation process shown is used to investigate the flotation behavior of ferric ion inhibitors under different pulp pH conditions through flotation experiments under different pH conditions.

[0025] The specific operation is as follows: Lithium mica and feldspar ore are crushed and ground to produce mineral samples with a particle size of 0.038~0.074mm. 2g of each sample is weighed and placed in a 40mL flotation cell, along with 35mL of deionized water and a pH adjuster (hydrochloric acid or sodium hydroxide). The slurry is adjusted to a specific pH (2, 4, 6, 8, 10) and stirred for 2 minutes. Then, a ferric ion inhibitor and a collector are added sequentially, with the inhibitor ferric chloride hexahydrate used at a dosage of 1.5 × 10⁻⁶. -4 After stirring for 3 minutes, add the collector (dodecylamine at a concentration of 1 × 10⁻⁶ mol / L). -4 (mol / L), after stirring for 3 minutes, aeration and foam scraping were started. The collected foam product and the product in the tank were filtered, dried and weighed separately. The recovery rate was calculated, and the results are shown in Table 3.

[0026] Table 3 Fe 3+ Inhibitor recovery rate at different pH levels

[0027] As shown in Table 3, the recovery rate of lepidolite is higher than that of feldspar in the pH range of 2-10. In particular, at pH=6, the flotation difference between lepidolite and feldspar reaches 77%, indicating that the inhibitor has the ability to efficiently separate particles even when the pulp pH is close to neutral.

[0028] Comparative Example 1 Other conditions are the same as in Example 1, except that Fe was not added. 3+ Inhibitors, and the results are shown in Table 4.

[0029] Table 4. Fe-free 3+ Recovery rate at different pH values

[0030] As shown in Table 4, both lepidolite and feldspar achieved high recovery rates within a pH range of 2-10, and there was no significant difference in flotation between the two minerals.

[0031] Comparative Example 2 The other conditions were the same as in Example 1, except that a sodium hexametaphosphate inhibitor was used. The results are shown in Table 5.

[0032] Table 5. Recovery rates of sodium hexametaphosphate inhibitors at different pH values.

[0033] As shown in Table 5, the flotation difference between lepidolite and feldspar is relatively small within the pH range of 2-10. The largest difference, reaching 62%, is observed at pH=2. However, the flotation environment of strong acid causes significant corrosion to the equipment, which is detrimental to actual production.

[0034] Comparative Example 3 The other conditions were the same as in Example 1, except that a water glass inhibitor was used. The results are shown in Table 6.

[0035] Table 6. Recovery rates of water glass inhibitors at different pH values

[0036] As shown in Table 6, the flotation differences between lepidolite and feldspar are relatively small within the pH range of 2-10. The largest difference, reaching 68%, is observed at pH=2. However, the flotation environment of strong acid causes significant corrosion to the equipment, which is detrimental to actual production.

[0037] Example 2 The actual lepidolite ore used in this embodiment has the following main mineral composition: Mineral composition Feldspar quartz Lithium mica Kaolinite apatite content / % 56.19 18.16 18.08 5.77 1.80 Flotation adopts Figure 2 The process is shown below.

[0038] The specific operation is as follows: 200g of actual ore is wet-milled using a ball mill so that the proportion of -0.074mm is about 90%; after desliming, it is poured into a 0.75L flotation cell, an appropriate amount of water is added and the pH is adjusted to 6, and then the metal ion inhibitor and collector described in this case are added in sequence, stirred for 3 minutes, and the foam is scraped for 5 minutes. A closed-loop flotation process was implemented, consisting of one roughing stage (ferric chloride hexahydrate added at 300-600 g / t, dodecylamine added at 160-240 g / t), one cleaning stage (ferric chloride hexahydrate added at 75-150 g / t), and one scavenging stage (ferric chloride hexahydrate added at 150-300 g / t, dodecylamine added at 80-120 g / t). The middlings were sequentially returned to the roughing stage. The concentrate was scraped to the concentrate basin along with the froth, while the tailings remained in the flotation cell. Both the concentrate and tailings were filtered, dried, and weighed separately. The grade of the concentrate was tested, and the recovery rate was calculated. K, X, N, and Y represent the concentrate, tailings, slime, and calculated raw ore, respectively. Table 7 shows the grade and recovery rate results for Example 2.

[0039] Table 7 Flotation results of Example 2

[0040] As shown in Table 7, the grade of lepidolite concentrate is only 0.91% when ferric chloride is not added. As the dosage of the inhibitor increases from 200 g / t to 400 g / t, the grade and recovery rate of lepidolite increase significantly. In particular, at 400 g / t, the grade of LiO2 reaches about 2.36% and the recovery rate reaches about 71%. For low-grade lepidolite ore, the metal ion inhibitor of this invention has strong selective collection performance of lepidolite in actual lepidolite ore.

[0041] Comparative Example 4 Using the actual lepidolite ore from Example 2, a roughing, cleaning, and scavenging flotation process was conducted with a common descaling agent. The specific operation was as follows: 200g of the actual ore was wet-milled using a ball mill to achieve a -0.074mm fraction of approximately 90%. After desliming, the ore was poured into a 0.75L flotation cell, and an appropriate amount of water was added to adjust the pH to 6. Then, sodium hexametaphosphate / water glass descaling agent and collector were added sequentially, stirred for 3 minutes, and foam scraping was initiated for 5 minutes. A closed-loop flotation process was implemented, consisting of 1 roughing stage (2000 g / t of sodium hexametaphosphate / water glass and 200 g / t of dodecylamine), 4 cleaning stages (1000 g / t, 500 g / t, 300 g / t, and 100 g / t of sodium hexametaphosphate / water glass respectively), and 1 scavenging stage (500 g / t of sodium hexametaphosphate / water glass and 80 g / t of dodecylamine). The middlings were sequentially returned to the roughing stage. The concentrate was scraped to the concentrate basin along with the froth, while the tailings remained in the flotation cell. Both the concentrate and tailings were filtered, dried, and weighed separately. The grade of the concentrate was tested, and the recovery rate was calculated. K, X, N, and Y represent the concentrate, tailings, slime, and calculated raw ore, respectively. Table 8 shows the grade and recovery rate results for Example 2.

[0042] Table 8 Flotation results of Comparative Example 2

[0043] Table 8 shows that when sodium hexametaphosphate and water glass are used as inhibitors, the grade of lepidolite concentrate is only 1.78% and 1.92%, respectively. Compared to Fe... 3+ The grade is relatively low, and the flotation performance is relatively poor.

[0044] The preferred embodiments of the present invention have been described in detail above with reference to the examples. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0045] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0046] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A flotation method for lepidolite, characterized in that, Includes the following steps: S1. Adjust the pH of the roughing concentrate slurry to 4-8, and add Fe sequentially. 3+ And the collector dodecylamine, Fe 3+ The reagent was added at a rate of 300-600 g / t, followed by aeration and foam scraping to obtain roughing froth products and scavenging feed, respectively. S2. Add Fe to the scavenged feed obtained in step S1. 3+ And the collector dodecylamine, Fe 3+ The reagent is added at a rate of 150~300g / t, and aeration and foaming are carried out to obtain scavenging foam products and tailings; S3. Adjust the pH of the coarse foam product obtained in step S1 and the scavenging foam product obtained in step S2 to 4-8, and add Fe. 3+ The addition amount is 75~150g / t, followed by aeration and foam removal to obtain lepidolite concentrate; Soluble iron salts were prepared into solutions with a mass concentration of 1% to 3% as Fe 3+ Add reagents.

2. The flotation method for lepidolite according to claim 1, characterized in that, In step S1, the method for obtaining the concentrate slurry is as follows: the raw ore is wet-milled and then deslimed to obtain the roughing concentrate slurry.

3. The flotation method for lepidolite according to claim 2, characterized in that, The raw ore has a Li2O grade of 0.8% to 0.9%, and the desliming amount is 5% to 8%.

4. The flotation method for lepidolite according to claim 1, characterized in that, The amount of dodecylamine added in step S1 is 160~240g / t, and the amount of dodecylamine added in step S2 is 80~120g / t.

5. The flotation method for lepidolite according to claim 4, characterized in that, In steps S1 to S2, the collector is a mixture of dodecylamine and hydrochloric acid / acetic acid.

6. The flotation method for lepidolite according to claim 1, characterized in that, During the flotation process, the temperature of the pulp is 5~50℃.

Citation Information

Patent Citations

  • Novel lepidolite floating selecting method, collecting agent and application thereof

    CN104741245A