Grain orientation random single-phase high-entropy alloy sheet processing method
By combining hot forging with multi-pass bidirectional cross-rolling, the problem of random grain orientation in large-size high-entropy alloy plates was solved, improving yield and reducing cost, thus enabling the industrial application of high-entropy alloy plates.
Patent Information
- Application Number
- CN202410022126.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-08
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-01-08
AI Technical Summary
Existing technologies make it difficult to process large-size high-entropy alloy plates and to ensure random grain orientation, which affects their application in the field of structural materials.
By combining hot forging with multi-pass bidirectional cross-rolling, alloy composition and heat treatment parameters are determined using Thermo Calc software, and real-time monitoring is performed using an infrared thermometer to gradually eliminate forging defects and ensure random grain orientation.
This improved the yield of single-phase high-entropy alloy plates, reduced costs, and enabled the industrial production of large-size high-entropy alloy plates.
Smart Images

Figure CN117753814B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal alloy material processing technology, specifically relating to a method for processing single-phase high-entropy alloy plates with random grain orientation. Background Technology
[0002] High-entropy alloys are a type of multi-principal-element alloy, a novel class of alloy materials developed in recent years. They typically contain at least four main metallic elements, with the content of each element designed according to equiatomic or non-equiatomic ratios, and the atomic content of each main element should not be less than 5%. Unlike traditional alloy materials, high-entropy alloys have high mixing entropy, making them less prone to forming intermetallic compounds and more likely to form solid solution structures. High-entropy alloys also possess unique characteristics in terms of kinetics, microstructure, and properties compared to traditional alloys, making them a metallic material with excellent comprehensive performance and great application prospects.
[0003] Plate materials, as one of the most common structural forms, are widely used in military, aerospace, shipbuilding, and engineering equipment fields. To fully utilize the excellent comprehensive properties of high-entropy alloy plates, it is necessary to ensure the alloy's isotropy, that is, to guarantee the random orientation of the alloy's grains. Currently, for large-size high-entropy alloys, processing them into isotropic high-entropy alloy plates with random grain orientation is of great significance for promoting the application of high-entropy alloys in the field of structural materials. Summary of the Invention
[0004] The technical problem to be solved by this invention is to provide a method for processing single-phase high-entropy alloy sheets with random grain orientation, addressing the shortcomings of the prior art. This method determines the hot forging and heat treatment processes based on the high-entropy alloy composition and processing dimensions, and combines hot forging with a multi-pass bidirectional cross-rolling process. This reduces microstructural defects in the single-phase high-entropy alloy sheets, ensures random grain orientation, and improves the yield of single-phase high-entropy alloy sheets.
[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: a method for processing single-phase high-entropy alloy plates with random grain orientation, wherein the single-phase high-entropy alloy is a CoCrFeNiAlTi system high-entropy alloy, characterized in that the method includes the following steps: Step 1: Three-fire forging Step 101: First-stage hot forging: Calculate the phase diagram of the CoCrFeNiAlTi high-entropy alloy using Thermo Calc software and determine the single-phase temperature range. Combined with the dimensions of the cylindrical high-entropy alloy ingot, hold the cylindrical high-entropy alloy ingot at a furnace temperature of 1050℃~1200℃ for 1h~3h. Use a free forging hydraulic press to forge once along each of the two mutually perpendicular radial directions of the cylindrical high-entropy alloy ingot, with a reduction of 15%~25% for each forging. Forge four planes on the cylindrical surface of the cylindrical high-entropy alloy ingot. Then, compress twice along the height direction of the cylindrical high-entropy alloy ingot, with a reduction of 3%~8% for each compression. Finally, flatten the cylindrical surface to minimize the arc surface, obtaining the first-stage forging. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object in real time. Forging is stopped when the surface temperature of the object drops to 920°C. If there is no obvious crack on the surface, it is returned to the furnace for heating. If there is obvious crack on the surface, the cracked part is cut off after cooling in the air and then returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1050℃~1200℃ for 0.5h, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence, with a reduction of 10%~20% for each forging, to obtain a second-stage forging with a square cross-section. During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1050℃~1200℃ for 0.5h. Then, three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and the reduction amount of each length forging is 5%~10%. The parts are air-cooled to room temperature to obtain the three-heat forging. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy sheet, the three-fired forging obtained in Step 103 is cut into master stock. Then, the master stock is subjected to multi-pass bidirectional cross-rolling using a hot and cold rolling mill. The number of passes in the multi-pass bidirectional cross-rolling is 4 to 8, and the deformation per pass is 5% to 15%, to obtain the rolled sheet. When large cracks appear at the edge of the master stock during the multi-pass bidirectional cross-rolling process, the cracked part is removed using a sheet metal machine. Step 3, Heat treatment: The rolled plate obtained in step 2 is subjected to vacuum annealing heat treatment at 950℃~1200℃ for 0.5h~1h, cooled in the furnace, leveled by a leveling machine, and then laser-cut to the target size of the single-phase high-entropy alloy plate. After polishing, the single-phase high-entropy alloy plate is obtained.
[0006] The above-described method for processing single-phase high-entropy alloy plates with random grain orientation is characterized in that the cylindrical high-entropy alloy ingot in step one has a diameter of 100 mm or more and a height-to-diameter ratio of 1 or more. Further, the cylindrical high-entropy alloy ingot has a diameter of 150 mm or more and a height-to-diameter ratio of 1.5 or more. By limiting the height-to-diameter ratio of the cylindrical high-entropy alloy ingot, bending of the forging during hot forging is prevented.
[0007] The above-mentioned method for processing single-phase high-entropy alloy plates with random grain orientation is characterized in that the cylindrical high-entropy alloy ingot in step one has an FCC single-phase structure with random grain orientation.
[0008] The above-mentioned method for processing single-phase high-entropy alloy plates with random grain orientation is characterized in that the heat preservation time in step 101 is 1h to 3h, the reduction amount of each forging in the first forging is 15% to 25%, and the reduction amount of each compression in the second compression is 3% to 8%.
[0009] The above-mentioned method for processing a single-phase high-entropy alloy sheet with random grain orientation is characterized in that the heat preservation time in step 102 is 0.5h, and the reduction amount of each forging is 10%~20%.
[0010] The above-mentioned method for processing single-phase high-entropy alloy plates with random grain orientation is characterized in that the heat preservation time in step 103 is 0.5h, and the reduction amount of each fixed-length forging is 5%~10%.
[0011] The above-mentioned method for processing single-phase high-entropy alloy plates with random grain orientation is characterized in that the number of passes in the multi-pass bidirectional cross rolling in step two is 4 to 8, and the deformation amount per pass is 5% to 15%.
[0012] Compared with the prior art, the present invention has the following advantages: 1. This invention targets CoCrFeNiAlTi series high-entropy alloys. The phase diagram of the high-entropy alloy composition is calculated using Thermo Calc software, and the single-phase temperature range is determined. Based on the alloy composition and ingot / forging dimensions, the temperature and time for hot forging and heat treatment are determined, thereby obtaining single-phase high-entropy alloy plates.
[0013] 2. This invention combines hot forging with multi-pass bidirectional cross rolling process to promptly eliminate forging defects, reduce microstructural defects in single-phase high-entropy alloy plates, and ensure random grain orientation, thereby improving the yield of single-phase high-entropy alloy plates and reducing overall costs, thus realizing the preparation of industrial-grade large-size single-phase high-entropy alloy plates.
[0014] 3. The processing method of this invention has a clear concept, is simple to operate, safe and reliable, economical and efficient, and is conducive to the industrial promotion and application of high-entropy alloy plates.
[0015] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0016] Figure 1 Co in Embodiment 1 of the present invention 30 Cr 20 Fe 25 Ni 15 The content of each phase in Al7Ti3 high-entropy alloy varies with temperature.
[0017] Figure 2a This is a physical image of the single-phase high-entropy alloy plate prepared in Example 1 of the present invention, taken in the width direction.
[0018] Figure 2b This is a physical image of the single-phase high-entropy alloy plate prepared in Example 1 of the present invention along its length.
[0019] Figure 3 The image shows the X-ray diffraction pattern of the single-phase high-entropy alloy plate prepared in Example 1 of this invention.
[0020] Figure 4 This is a microstructure diagram of the single-phase high-entropy alloy plate prepared in Example 1 of the present invention.
[0021] Figure 5 The figure shows the tensile properties of the single-phase high-entropy alloy sheet prepared in Example 1 of this invention. Detailed Implementation
[0022] Example 1 This embodiment includes the following steps: Step 1: Three-fire forging Step 101, Hot Forging: Calculate Co using Thermo Calc software. 30 Cr 20 Fe 25 Ni 15 The changes in phase fractions with temperature in Al7Ti3 high-entropy alloys, such as... Figure 1 As shown, from Figure 1 It can be seen that as the temperature decreases, the alloy transforms from a liquid state to an FCC solid phase. When the temperature is below 620℃, BCC phase, Sigma phase and Ni3Ti phase appear. Therefore, it is determined that the alloy has an FCC single-phase structure in the temperature range of 620℃~1370℃. A cylindrical Co with a diameter of 186mm and a height of 255mm 30 Cr 20 Fe25 Ni 15 Al7Ti3 high-entropy alloy ingots were held at 1150℃ for 1.5 hours in a furnace. Then, a free forging hydraulic press was used to forge the cylindrical high-entropy alloy ingots once along two mutually perpendicular radial directions, with a reduction of 20%~25% for each forging. Initially, four planes were forged on the cylindrical surface of the cylindrical high-entropy alloy ingots. Then, the ingots were compressed twice along their height, with a reduction of 3%~8% for each compression. Finally, the cylindrical surface was flattened to minimize the arc surface, resulting in a quasi-rectangular forging with a length × width × height of 180mm × 170mm × 210mm. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1150℃ for 0.5h, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence, with a reduction of 10%~18% for each forging, to obtain a second-stage forging with a length × width × height of 200mm × 200mm × 155mm and a square cross-section; During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1150℃ for 0.5h. Then, three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and the reduction amount of each length forging is 5%~10%. After air cooling to room temperature, a three-heat forging with a length × width × height of 220mm × 220mm × 127mm is obtained. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy plate, the three-fire forging obtained in step 103 is cut into a master material with a length × width × thickness of 200mm × 200mm × 15mm. Then, the master material is subjected to 8 passes of bidirectional cross-rolling using a hot and cold rolling mill, with a single pass deformation of 0.8mm~2.2mm, to obtain a rolled plate with a length × width × thickness of 321mm × 320mm × 5.1mm. Step 3, Heat Treatment: The rolled sheet obtained in Step 2 is subjected to vacuum annealing heat treatment at 1150℃ for 1 hour, followed by furnace cooling. It is then leveled using a leveling machine, laser-cut, and polished to obtain a single-phase high-entropy alloy sheet with a length × width × thickness of 300mm × 300mm × 5mm and random grain orientation. Figure 2a and Figure 2b As shown.
[0023] Figure 3 The X-ray diffraction pattern of the single-phase high-entropy alloy plate prepared in this embodiment is shown below. Figure 3 It can be seen that the single-phase high-entropy alloy plate is a face-centered cubic single phase.
[0024] Figure 4 This is a microstructure diagram of the single-phase high-entropy alloy plate prepared in this embodiment. Figure 3 It can be seen that the grain orientation of this single-phase high-entropy alloy plate is random.
[0025] Figure 5 This is a graph showing the tensile properties of the single-phase high-entropy alloy sheet prepared in this embodiment. Figure 5 It can be seen that the yield strength of this single-phase high-entropy alloy plate is 700 MPa and the tensile strength is 975 MPa.
[0026] Example 2 This embodiment includes the following steps: Step 1: Three-fire forging Step 101, Hot Forging: Calculate Co using Thermo Calc software. 30 Cr 20 Fe 25 Ni 15 The phase fractions of the Al7Ti3 high-entropy alloy varied with temperature, determining that the alloy exhibited an FCC single-phase structure within the temperature range of 620℃ to 1370℃. A cylindrical Co-shaped sample with a diameter of 135mm and a height of 220mm was used. 30 Cr 20 Fe 25 Ni 15 Al7Ti3 high-entropy alloy ingots were held at 1150℃ for 1 hour in a furnace. Then, a free forging hydraulic press was used to forge the cylindrical high-entropy alloy ingots once along two mutually perpendicular radial directions, with a reduction of 15%~25% for each forging. Initially, four planes were forged on the cylindrical surface of the cylindrical high-entropy alloy ingots. Then, the ingots were compressed twice along the height direction, with a reduction of 3%~8% for each compression. Cracks with a thickness of more than 2mm were found on the original cylindrical end face. After air cooling to room temperature, the cracked parts were removed, and the ingots were reheated and held at 1 hour in the furnace. The cylindrical surface was then flattened to minimize the arc surface, resulting in a quasi-rectangular forging with a length × width × height of 133mm × 135mm × 150mm. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1150℃ for 0.5h, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence, with a reduction of 15%~20% for each forging, to obtain a second-stage forging with a length×width×height of 152mm×150mm×112mm and a square cross-section; During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1150℃ for 0.5h. Then, three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and the reduction amount of each length forging is 5%~10%. After air cooling to room temperature, a three-heat forging with a length × width × height of 160mm × 160mm × 85mm is obtained. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy sheet, the three-fire forging obtained in step 103 is cut into a master material with a length × width × thickness of 160mm × 160mm × 10mm. Then, the master material is subjected to four passes of bidirectional cross-rolling using a hot and cold rolling mill, with a single pass deformation of 0.5mm to 1.5mm. During the third pass of rolling, a 2cm long crack appears at the edge. After being removed by a sheet metal machine, it is rolled for one more pass to obtain a rolled sheet with a length × width × thickness of 202mm × 205mm × 5.08mm. Step 3, Heat treatment: The rolled plate obtained in Step 2 is subjected to vacuum annealing heat treatment at 1150℃ for 0.5h, cooled in the furnace, leveled by a leveling machine, then laser-cut and polished to obtain a single-phase high-entropy alloy plate with a length × width × thickness of 200mm × 200mm × 5mm and random grain orientation.
[0027] Example 3 This embodiment includes the following steps: Step 1: Three-fire forging Step 101, Hot Forging: Calculate Co using Thermo Calc software. 37 Cr 16 Fe 25 Ni 16 The phase fractions of the Al4Ti2 high-entropy alloy varied with temperature, determining that the alloy exhibited an FCC single-phase structure within the temperature range of 620℃ to 1375℃. A cylindrical Co sample with a diameter of 136mm and a height of 225mm was then used. 37 Cr 16 Fe 25 Ni 16Al4Ti2 high-entropy alloy ingots are held at 1200℃ for 2 hours in a furnace. A free forging hydraulic press is used to forge the cylindrical high-entropy alloy ingot once along two mutually perpendicular radial directions, with a reduction of 20%~25% for each forging. Initially, four planes are forged on the cylindrical surface of the cylindrical high-entropy alloy ingot. Then, the cylindrical high-entropy alloy ingot is compressed twice along the height direction, with a reduction of 3%~8% for each compression. The cylindrical surface is then flattened to eliminate the arc surface as much as possible, resulting in a one-fire forging of a quasi-rectangular block with a length × width × height of 135mm × 130mm × 180mm. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1200℃ for 0.5h, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence, with a reduction of 10%~18% for each forging, to obtain a second-stage forging with a length×width×height of 150mm×150mm×125mm and a square cross-section; During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1200℃ for 0.5h. Then, three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and the reduction amount of each length forging is 5%~10%. After air cooling to room temperature, a three-heat forging with a length × width × height of 160mm × 160mm × 105mm is obtained. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy sheet, the three-fired forging obtained in Step 103 is cut into a master stock with a length × width × thickness of 200mm × 200mm × 15mm. Then, the master stock is subjected to six passes of bidirectional cross-rolling using a hot and cold rolling mill, with a single pass deformation of 0.4mm to 1.1mm. During the fourth pass, a 1cm long crack appears at the edge. After being removed with a sheet metal machine, it is rolled for one more pass to obtain a rolled sheet with a length × width × thickness of 252mm × 250mm × 2.45mm. Step 3, Heat treatment: The rolled plate obtained in Step 2 is subjected to vacuum annealing heat treatment at 1200℃ for 1 hour, cooled in the furnace, leveled by a leveling machine, then laser-cut, and polished to obtain a single-phase high-entropy alloy plate with a length × width × thickness of 220mm × 220mm × 2.45mm and random grain orientation.
[0028] Example 4 This embodiment includes the following steps: Step 1: Three-fire forging Step 101, Hot Forging: Calculate Co using Thermo Calc software. 35 Cr 18 Fe 25 Ni 18 The phase fractions of the Al1Ti3 high-entropy alloy varied with temperature, determining that the alloy exhibited an FCC single-phase structure within the temperature range of 650℃ to 1350℃. A cylindrical Co-shaped sample with a diameter of 245mm and a height of 315mm was then used. 35 Cr 18 Fe 25 Ni 18 Al1Ti3 high-entropy alloy ingots were held at 1050℃ for 3 hours in a furnace. A free forging hydraulic press was used to forge the cylindrical high-entropy alloy ingot once along two mutually perpendicular radial directions, with a reduction of 15%~20% for each forging. Initially, four planes were forged on the cylindrical surface of the cylindrical high-entropy alloy ingot. Then, the ingot was compressed twice along its height, with a reduction of 3%~8% for each compression. Cracks with a thickness of more than 2mm were found on the original cylindrical end face plane. After air cooling to room temperature, the cracked parts were removed, and the ingot was reheated and held at 3 hours in the furnace. The cylindrical surface was then flattened to minimize the arc surface, resulting in a quasi-rectangular forging with a length × width × height of 203mm × 200mm × 305mm. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1050℃ for 0.5h, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence, with a reduction of 10%~18% for each forging, to obtain a second-stage forging with a length×width×height of 210mm×210mm×275mm and a square cross-section. During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1500℃ for 0.5h. Then, three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and the reduction amount of each length forging is 5%~10%. After air cooling to room temperature, a three-heat forging with a length × width × height of 215mm × 215mm × 260mm is obtained. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy plate, the three-fire forging obtained in step 103 is cut into a master material with a length × width × thickness of 215mm × 215mm × 27mm. Then, the master material is subjected to six passes of bidirectional cross-rolling using a hot and cold rolling mill, with a single pass deformation of 1.4mm to 4mm, to obtain a rolled plate with a length × width × thickness of 320mm × 320mm × 9.9mm. Step 3, Heat treatment: The rolled plate obtained in Step 2 is subjected to vacuum annealing heat treatment at 950℃ for 1 hour, cooled in the furnace, leveled by a leveling machine, then laser-cut, and polished to obtain a single-phase high-entropy alloy plate with a length × width × thickness of 300mm × 300mm × 9.9mm and random grain orientation.
[0029] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.
Claims
1. A method for processing a single-phase high-entropy alloy sheet with random grain orientation, the single-phase high-entropy alloy being a CoCrFeNiAlTi-based high-entropy alloy, characterized in that, The method includes the following steps: Step 1: Three-fire forging Step 101: Hot Forging: Calculate the phase diagram of the CoCrFeNiAlTi high-entropy alloy using Thermo Calc software and determine the single-phase temperature range. Combined with the dimensions of the cylindrical high-entropy alloy ingot, hold the ingot at a furnace temperature of 1050℃~1200℃. Use a free forging hydraulic press to forge the ingot once along each of its two mutually perpendicular radial directions, forging four planes on the cylindrical surface. Then, compress the ingot twice along its height direction. Finally, flatten the cylindrical surface to minimize the arc surface, resulting in a hot-forged part. The cylindrical high-entropy alloy ingot has an FCC single-phase structure with random grain orientation. The heat preservation time is 1 hour to 3 hours, the reduction amount of each forging in the first forging is 15% to 25%, and the reduction amount of each compression in the second compression is 3% to 8%. During the forging and compression process, an infrared thermometer is used to measure the surface temperature of the object in real time. Forging is stopped when the surface temperature of the object drops to 920°C. If there is no obvious crack on the surface, it is returned to the furnace for heating. If there is obvious crack on the surface, the cracked part is cut off after cooling in the air and then returned to the furnace for heating. Step 102, Second-stage hot forging: The first-stage forging obtained in step 101 is held at a furnace temperature of 1050℃~1200℃, and then the three pairs of parallel surfaces in the first-stage forging are forged in sequence to obtain a second-stage forging with a square cross-section. During the forging process, an infrared thermometer is used to measure the surface temperature of the object being processed in real time. Forging is stopped when the surface temperature of the object being processed drops to 920°C, and the object is returned to the furnace for heating. Step 103, Three-heat hot forging: The two-heat forging obtained in step 102 is held at a furnace temperature of 1050℃~1200℃, and then the three pairs of mutually perpendicular parallel surfaces in the two-heat forging are forged to length in sequence, and air-cooled to room temperature to obtain the three-heat forging. Step 2, Bidirectional Cross-rolling: Based on the volume of the target single-phase high-entropy alloy sheet, the three-fired forging obtained in Step 103 is cut into master stock. Then, the master stock is subjected to multi-pass bidirectional cross-rolling using a hot and cold rolling mill to obtain the rolled sheet. During the multi-pass bidirectional cross-rolling process, if large cracks appear at the edge of the master stock, the cracked portion is removed using a sheet metal machine. The number of passes in the multi-pass bidirectional cross-rolling is 4-8, and the deformation per pass is 5%-15%. Step 3, Heat treatment: The rolled plate obtained in step 2 is subjected to vacuum annealing heat treatment at 950℃~1200℃ for 0.5h~1h, cooled in the furnace, leveled by a leveling machine, and then laser-cut to the target size of the single-phase high-entropy alloy plate. After polishing, the single-phase high-entropy alloy plate is obtained.
2. The method of claim 1, wherein the method is characterized by: The cylindrical high-entropy alloy ingot mentioned in step one has a diameter of 100 mm or more and a height-to-diameter ratio of 1 or more.
3. The method of claim 1, wherein the method is characterized by: The heat preservation time mentioned in step 102 is 0.5h, and the reduction amount of each forging is 10%~20%.
4. The method of claim 1, wherein the method is characterized by: The heat preservation time in step 103 is 0.5h, and the reduction amount of each fixed-length forging is 5%~10%.
Citation Information
Patent Citations
Processing technology of large-size high-strength magnesium alloy sheet
CN102586561A
Ultrahigh strength-plasticity matched high-entropy alloy and preparation method thereof
CN115449691A