A combined welding method for improving the gas-tight reliability of a radio-frequency connector weld
By combining reflow soldering and induction soldering, the problem of residual flux after welding of RF connectors is solved, improving the airtightness, reliability and aesthetics of the weld, and making it suitable for mass production of microwave components.
Patent Information
- Application Number
- CN202410159642.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-02-04
AI Technical Summary
Residual flux after soldering of RF connectors affects the long-term airtightness and reliability of the components, and existing soldering methods cannot effectively solve this problem.
A combined welding method of reflow soldering and induction welding is adopted. First, reflow soldering is used to reduce flux residue, and then the weld is heated by the induction welding coil to make the residual flux overflow. Solvent cleaning is combined to ensure the airtightness of the weld.
It significantly improves the airtightness, reliability, and aesthetics of RF connector welds, increases processing efficiency, overcomes the shortcomings of a single welding method, and is suitable for mass production and localized adjustment of weld quality.
Smart Images

Figure CN117754067B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of microwave component microelectronic welding technology, specifically to a combined welding method for improving the airtight reliability of RF connector welds. Background Technology
[0002] The weld seams of RF connectors are typically narrow and deep. After soldering, flux often cannot completely overflow and remains in the weld seam, clogging the pores. Cleaning cannot effectively remove it completely, which interferes with the weld seam airtightness screening results and affects the long-term airtightness reliability of the components.
[0003] Currently, no single welding method can effectively address this issue: reflow oven welding and vapor phase welding are mature processes with high efficiency for mass production of components, and adjustable parameters can result in good overall welding results for multiple components, but the adjustment effect for a single weld seam is generally limited; hot plate welding is relatively rough, with relatively poor weld formation, and the overall effect is not as good as reflow welding; induction welding can weld a single weld seam, but the temperature rise is relatively fast, and it is easy to burn the connector when used alone, and the welding time is shorter than reflow welding, making it more difficult to remove residual flux.
[0004] Reducing the amount of flux used can mitigate the impact of residual flux clogging pores on airtightness screening results. However, currently used flux coating methods cannot effectively solve this problem: manual flux application cannot precisely and evenly control the flux dosage, and insufficient application can lead to poor solder wetting and poor weld formation; machine spraying requires additional equipment, increasing costs, and the porous structure of some components makes automated flux spraying unsuitable; using pre-coated flux solder is one solution, but it requires custom-designed flux and solder combinations, multiple trials to determine the correct ratio, a lengthy process, and increased costs. The search is for a type of flux that leaves no residue after soldering, but currently, no ideal and economical flux has been found to achieve this goal, especially for RA or RMA type fluxes with high-reliability weld requirements.
[0005] To address the aforementioned shortcomings, this invention proposes a combined welding method to improve the airtight reliability of RF connector weld seams. Summary of the Invention
[0006] The technical problem to be solved by this invention is: how to solve the problem of flux residue after soldering of RF connectors.
[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0008] A combined welding method for improving the hermeticity reliability of RF connector weld seams includes the following steps:
[0009] S1. Solder the RF connector using reflow soldering by using tin-lead or lead-free solder that requires flux.
[0010] S2. Use solvent to clean the RF connector assembly and remove the flux from the solder joint surface;
[0011] S3. Then, adjust the shape of the induction coil according to the RF connector assembly, and use induction welding to heat the RF connector weld seam without flux, so that the RF connector weld seam melts and overflows the remaining flux.
[0012] S4. Clean the RF connector assembly again with solvent to remove any excess flux.
[0013] This invention optimizes the reflow soldering process by minimizing flux residue. Then, an induction soldering coil briefly melts the RF weld seam, causing any remaining flux to escape. This eliminates potential hermetic failures in components from the initial assembly stage, improving long-term hermetic reliability. The combined reflow and induction soldering processes offer complementary advantages while avoiding the drawbacks of individual methods. Reflow soldering is a mature and efficient process, capable of simultaneously soldering multiple RF connectors, making it suitable for mass production. However, it cannot provide targeted intervention for individual weld seams. Induction soldering, on the other hand, provides rapid and concentrated heating, allowing for adjustments to specific weld seams. Reflow soldering ensures efficiency, while induction soldering improves weld quality, significantly enhancing hermetic reliability.
[0014] As a further aspect of the present invention: in step S1, the solder used is either tin-lead or lead-free and requires the use of flux, but is not limited to solder rings, solder wires, or solder paste.
[0015] As a further aspect of the present invention: the flux is selected as a rosin-based flux, and the flux is applied by, but not limited to, manual coating or machine spraying, and the activity of the flux is selected by, but not limited to, RA type or RMA type.
[0016] As a further aspect of the present invention, the reflow soldering in step S1 may employ, but is not limited to, a vacuum reflow oven or a nitrogen reflow oven.
[0017] As a further aspect of the present invention: the radio frequency connector in step S1 is, but is not limited to, an SMP miniature pluggable connector.
[0018] As a further aspect of the present invention: the solvent in step S2 is, but is not limited to, bromopropane or anhydrous ethanol, an azeotropic solvent composed of hydrophobic, hydrophilic, or a mixture of hydrophobic and hydrophilic types.
[0019] As a further aspect of the present invention: the parameters for induction welding in step S3 are as follows: output power of 20%-70%, preheating temperature of 120-150℃, preheating time of 5-10s, welding temperature of 190-240℃, welding time of 10-25s, postheating of 70-100℃, postheating time of 3-5s, followed by cooling at room temperature.
[0020] As a further aspect of the present invention: in step S3, the shape of the induction welding coil is consistent with the shape of the weld, and is not limited to circular, square or elliptical, and the size of the coil is 3-15mm larger than the dimensions of the weld.
[0021] As a further aspect of the present invention, the cleaning in steps S2 and S4 is carried out by, but not limited to, automatic cleaning by a cleaning machine or manual cleaning.
[0022] As a further aspect of the present invention: the solvent in step S4 is, but is not limited to, bromopropane or anhydrous ethanol, an azeotropic solvent composed of hydrophobic, hydrophilic, or a mixture of hydrophobic and hydrophilic types.
[0023] Compared with the prior art, the beneficial effects of the present invention are:
[0024] I. This invention, through the rational design of the reflow soldering process, ensures as little flux residue as possible, and then uses an induction soldering coil to reheat the radio frequency weld seam to briefly melt it, causing the flux residue hidden in the weld seam to overflow due to heat. This can eliminate components with potential airtightness failure in the initial stage of the component, thereby improving the long-term airtightness reliability of the component.
[0025] Second, the present invention has high processing efficiency, the reflow soldering process is suitable for mass production, and the induction welding can locally and rapidly heat the weld seam with concentrated heat, and can complete the heating of a specific weld seam in 20-50 seconds.
[0026] Third, this invention overcomes the shortcomings of a single welding method and combines the advantages of two welding methods. Reflow soldering is suitable for mass production, but it cannot provide targeted intervention for individual welds, especially when multiple components are reflowed at the same time, it cannot effectively adjust only the RF connector welds. Induction soldering can adjust the size and shape of the induction coil and perform short-term heating adjustment on the RF connector welds. The heating time is much shorter than that of single induction soldering, which can protect the connector from damage caused by prolonged heating and greatly reduce the impact of induction soldering heating on the welds of other components.
[0027] IV. This invention has high reliability and significant effects. The reflow soldering process is mature and stable, the weld reliability is relatively high and the flux residue after welding is relatively small. The induction welding adjusts the weld and the heating time is shorter than that of welding connectors using induction welding alone. The flux remaining in the weld will overflow in a very short time when heated, greatly improving the weld reliability.
[0028] Fifth, the weld of the present invention is more aesthetically pleasing. The weld after combined welding is more continuous and bright, and is more aesthetically pleasing than the weld after a single welding method. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of an induction welding process according to an embodiment of the present invention;
[0030] Figure 2 This is an embodiment of the present invention. Figure 1 The front view;
[0031] Figure 3 This is an embodiment of the present invention. Figure 1 Top view;
[0032] Explanation of reference numerals in the attached diagram: 1. Induction welding coil; 2. RF connector weld seam; 3. Component housing. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] Example 1
[0035] Reference Figure 1-3 This invention utilizes a combined welding method to improve the airtightness reliability of RF connector welds, specifically for induction welding adjustment of vacuum reflow soldering welds in single-unit SMP RF connectors.
[0036] Step 1: A single-gang SMP RF connector is soldered using a vacuum reflow oven with a custom Sn63Pb37 solder ring and a certain RMA type flux. The vacuum reflow curve is a typical preheat-hold-reflow-cooling curve, and the vacuum extraction function is realized in the reflow zone. It should be noted that the vacuum reflow oven is a conventional device in the field, and this application only uses it without modification, so its principle will not be described in detail.
[0037] The preheating stage is from room temperature to 130℃, with a heating rate of 2℃ / s;
[0038] The heat preservation stage is from room temperature to 130℃-180℃, with a heating rate of 0.4℃ / s;
[0039] The peak temperature during the reflux phase was 215℃, and the reflux time was 55s.
[0040] The cooling phase is from cooling to 75℃, and the cooling rate is 3.5℃ / s.
[0041] Step 2: The RF connector assembly housing 3 is cleaned using an automatic vapor phase cleaner without ultrasonic function. The cleaning agent is bromopropane. The cleaning is repeated three times. Under a 40x microscope, it is confirmed that the flux on the surface of the RF connector solder joint has been cleaned. It should be noted that the automatic vapor phase cleaner is a conventional device in the field. This application only uses it without modification, so its principle will not be described in detail.
[0042] Step 3: The outer diameter of the weld seam of a single SMP RF connector is 3.9mm. Therefore, the induction welding coil 1 is adjusted to a circle with a diameter of 13mm, and the induction welding parameters are set as follows: output power of 30%, preheating temperature of 120℃, preheating time of 5s, welding temperature of 200℃, welding time of 25s, postheating temperature of 75℃, postheating time of 5s, and then placed in room temperature for cooling.
[0043] Induction soldering was used to heat the RF connector solder joint 2 without flux. As the solder melted, the connector was gently rotated in the solder using tweezers, and a glass rod was gently pressed into the center of the connector surface to ensure proper placement. A light yellow or yellowish-brown flux residue was observed to re-overflow from some of the solder joint surface.
[0044] Step 4: The RF connector assembly housing 3 is cleaned again using an automatic vapor phase cleaner without ultrasonic function. The cleaning agent is bromopropane. The cleaning is repeated three times. Then, it is confirmed under a 40x microscope that the flux on the surface of the RF connector solder joint has been cleaned. The initial air tightness test is qualified. It should be noted that the automatic vapor phase cleaner is a conventional equipment in the field. This application only uses it without modification, so its principle will not be described in detail.
[0045] Batch components (components refer to modular groups formed by soldering RF connectors to a metal housing through combination soldering, with each component containing 2 combination soldered RF connectors) underwent environmental screening tests. The specific screening test conditions are shown in Table 1 below. The combination soldered modular groups were tested and processed in sequence according to numbers 1-7 in the table and compared with the traditional single reflow soldered modular groups. The following conclusions were drawn: the airtightness pass rate of more than 1,000 components increased from the original 93.3% to 99.7%, indicating that the method is effective.
[0046] Table 1 Comparison of screening test results between combined welding and conventional welding connectors
[0047]
[0048]
[0049] Meanwhile, metallographic analysis was performed on a portion of the weld after induction welding. The thickness of the intermetallic compound increased from 1.52 μm after reflow welding to 2.12 μm, and the mixture was uniform and continuous, indicating that the welding quality met the requirements and the method was reliable.
[0050] The working principle of this invention is as follows:
[0051] The viscous residue left after soldering in rosin-based flux is rosin residue, a glassy and highly elastic polymer that is extremely difficult to completely remove with cleaning agents. However, after absorbing a certain amount of heat, it will revert to a liquid state and increase its flowability.
[0052] RF connector solder joints are typically narrow and deep. After soldering, flux often cannot completely overflow and remains in the solder joint, clogging pores. Cleaning cannot effectively remove this residue completely, interfering with the solder joint's airtightness test results. This allows components that were originally airtight to temporarily form a seal and pass the airtightness test. However, when the solder joint is subjected to environmental conditions exceeding room temperature, such as prolonged baking or thermal shock, the flux residue will overflow, leading to airtightness failure. This type of failure is insidious and delayed, severely impacting the long-term airtightness reliability of the component.
[0053] This invention first designs a reflow soldering process to minimize flux residue, and then uses an induction soldering coil to reheat the radio frequency weld seam briefly, causing the flux residue hidden in the weld seam to overflow. This eliminates components with potential airtightness failures at the initial stage of component development, thereby improving the long-term airtightness reliability of the components.
[0054] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A combined welding method for improving the hermetic reliability of RF connector weld seams, comprising the following steps: S1. Solder the RF connector using tin-lead or lead-free solder that requires flux, and then use reflow soldering. Select rosin-based flux with RA or RMA activity. S2. Use solvent to clean the RF connector assembly and remove the flux from the solder joint surface; S3. Then, adjust the shape of the induction coil according to the RF connector assembly, and use induction welding to heat the RF connector weld seam without flux. That is, the RF weld seam is heated again by the induction welding coil to briefly melt it, so that the flux residue hidden in the weld seam is heated and overflowed. The parameters of induction welding are: output power of 20%-70%, preheating temperature of 120-150℃, preheating time of 5-10s, welding temperature of 190-240℃, welding time of 10-25s, postheating of 70-100℃, postheating time of 3-5s, and then cooling at room temperature. S4. Clean the RF connector assembly again with solvent to remove any excess flux.
2. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The flux used is made of solder rings, solder wire, or solder paste.
3. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 2, characterized in that: The flux is applied manually or by machine spraying.
4. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The reflow soldering in step S1 uses a vacuum reflow oven or a nitrogen reflow oven.
5. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The RF connector in step S1 is an SMP miniature pluggable connector.
6. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The solvent in step S2 is an azeotropic solvent composed of bromopropane or anhydrous ethanol, which is hydrophobic, hydrophilic, or a mixture of hydrophobic and hydrophilic types.
7. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: In step S3, the shape of the induction welding coil is consistent with the shape of the weld, and it can be round, square or elliptical. The size of the coil is 3-15mm larger than the size of the weld.
8. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The cleaning in steps S2 and S4 can be done automatically by a cleaning machine or manually.
9. The combined welding method for improving the airtight reliability of RF connector weld seams according to claim 1, characterized in that: The solvent in step S4 is an azeotropic solvent composed of bromopropane or anhydrous ethanol, which is hydrophobic, hydrophilic, or a mixture of hydrophobic and hydrophilic types.
Citation Information
Patent Citations
Deep blind cavity radio frequency connector inner conductor welding structure and reflow soldering method
CN111541088A
Electromagnetic induction welding device
CN220073504U