A method for fabricating a micro-mechanical suspended structure using a common silicon substrate

By using two ordinary silicon substrates instead of SOI silicon wafers, and employing incomplete etching and wet etching methods to fabricate micromechanical suspended structures, the problems of high cost and difficult release of SOI silicon wafers are solved, enabling low-cost and simple suspended structure processing and high-precision sensor fabrication.

CN117756051BActive Publication Date: 2026-11-24XIAMEN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410050756.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2026-11-24
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

In existing technologies, the fabrication of micromechanical suspended structures using SOI silicon wafers suffers from high material costs, high processing costs, and difficulties in releasing the SiO₂ layer.

Method used

Two ordinary silicon substrates are used instead of SOI silicon wafers. A device layer with a micromechanical suspended structure is formed on the first ordinary silicon substrate by incomplete etching. After bonding with the second ordinary silicon substrate covered with a silicon nitride film, the suspended structure is released by wet etching to avoid adhesion problems.

Benefits of technology

This method enables low-cost and simple fabrication of micromechanical suspended structures, reduces processing difficulty, avoids adhesion problems between suspended structures, and improves the accuracy and applicability of sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117756051B_ABST
    Figure CN117756051B_ABST
Patent Text Reader

Abstract

This invention provides a method for fabricating micromechanical suspended structures using a conventional silicon substrate, comprising the following steps: selecting a conventional silicon substrate A, and obtaining multiple micromechanical suspended structures on the conventional silicon substrate A through incomplete etching, wherein the multiple micromechanical suspended structures are connected by an incompletely etched bottom interconnect layer; selecting a conventional silicon substrate B, and obtaining a support layer on the conventional silicon substrate B through complete etching; bonding the support layer of the conventional silicon substrate B to the multiple micromechanical suspended structures of the conventional silicon substrate A, so that the support layer simultaneously fixes the fixing areas of the multiple micromechanical suspended structures; and completely etching the bottom interconnect layer of the conventional silicon substrate A to separate the multiple micromechanical suspended structures; thus obtaining the micromechanical suspended structure. Using this method, a conventional silicon substrate can be used instead of an SOI silicon wafer to fabricate micromechanical suspended structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of microelectromechanical systems fabrication technology, and more specifically, relates to a method for fabricating micromechanical suspended structures using ordinary silicon substrates. Background Technology

[0002] With the development of microelectromechanical systems (MEMS) and the introduction of deep silicon etching processes, a series of MEMS device structures with high aspect ratio silicon structures have been realized. The use of silicon-on-insulator (SOI) technology has enabled further miniaturization and integration of MEMS devices, as shown in CN104118845B. However, there are several problems with fabricating MEMS devices based on SOI silicon wafers: First, commercially available SOI silicon wafers are expensive, the fabrication process is complex, and manufacturing thin SOI wafers is difficult; second, the use of SOI silicon wafers requires high precision in instruments and equipment, and sensors made from SOI silicon wafers have relatively high processing costs; third, when removing the SiO2 layer of the SOI silicon wafer through wet etching to release the suspended structure, the release is often difficult due to adhesion effects. Summary of the Invention

[0003] To address the aforementioned problems, this invention provides a method for fabricating micromechanical suspended structures using ordinary silicon substrates.

[0004] To achieve the above objectives, the technical solution provided by the present invention is as follows:

[0005] A method for fabricating micromechanical suspended structures using a common silicon substrate includes the following steps:

[0006] S1. Select a first ordinary silicon substrate and obtain multiple micromechanical suspended structures on the first ordinary silicon substrate through incomplete etching. The multiple micromechanical suspended structures constitute a device layer and are connected by an incompletely etched bottom interconnect layer. Each micromechanical suspended structure includes a fixed area and a cantilever structure connecting the fixed area. S2. Select a second ordinary silicon substrate covered with silicon nitride films on both sides and obtain a support layer through complete etching. S3. Bond the support layer obtained in step A2 and the device layer obtained in step S1 together, so that the support layer simultaneously fixes the fixed areas of multiple micromechanical suspended structures. S4. Completely etch the bottom interconnect layer of the first ordinary silicon substrate to separate the multiple micromechanical suspended structures; obtain the micromechanical suspended structure.

[0007] Further, step S1 specifically includes the following: S11, preparing a patterned protective layer of micromechanical suspended structure on the front side of the first ordinary silicon substrate to obtain silicon substrate A1; S12, performing deep silicon etching on the front side of silicon substrate A1, the etching does not penetrate the back side of silicon substrate A1 to obtain silicon substrate A2; S13, removing the patterned protective layer on the front side to obtain silicon substrate A3.

[0008] Furthermore, in step S12, etching is stopped when the depth of the etched area with the widest groove reaches 50%-80% of the total thickness of the first ordinary silicon substrate.

[0009] Further, step S2 specifically includes the following: S21, covering both sides of the second ordinary silicon substrate with silicon nitride films to obtain silicon substrate B1; S22, preparing a photoresist mask with a support layer pattern on the front side of silicon substrate B1 to obtain silicon substrate B2; S23, etching away the silicon nitride film exposed outside the photoresist mask on the front side of silicon substrate B2, and then removing the photoresist mask to obtain silicon substrate B3; S24, etching silicon substrate B3 to remove the silicon base layer without silicon nitride film coverage to obtain silicon substrate B4; S25, preparing a photoresist mask with a support layer pattern on the silicon nitride film on the bottom surface of silicon substrate B4, and etching it to obtain the support layer.

[0010] Further, step S24 is as follows: using a wet etching process, the silicon substrate B3 is placed in a KOH solution or a tetramethylammonium hydroxide solution to remove the silicon substrate without silicon nitride coverage on the silicon substrate B3, and then rinsed clean.

[0011] Furthermore, step S3 specifically includes the following: bonding the support layer obtained in S2 to the device layer obtained in S1 together using a bonding process; S32, completely etching the bottom interconnect layer of the first ordinary silicon substrate with the top facing upwards.

[0012] Furthermore, the thickness of the first and second ordinary silicon substrates is 50-500 μm.

[0013] The technical solution provided by this invention has the following beneficial effects:

[0014] This solution designs a method for fabricating micromechanical suspended structures using ordinary silicon wafers, enabling the use of ordinary silicon wafers to replace SOI silicon wafers in the fabrication of micromechanical suspended structures. This effectively solves the problems of high material costs, high processing costs, and difficulty in releasing the SiO2 layer when using SOI silicon wafers to fabricate micromechanical suspended structures. Attached Figure Description

[0015] Figure 1(a) shows a schematic diagram of the structure of the first ordinary silicon substrate in the embodiment;

[0016] Figure 1(b) shows a schematic diagram of the structure of silicon substrate A1 in the embodiment;

[0017] Figure 1(c) shows a schematic diagram of the structure of silicon substrate A2 in the embodiment;

[0018] Figure 1(d) shows a schematic diagram of the structure of silicon substrate A3 in the embodiment;

[0019] Figure 2(a) shows a schematic diagram of the structure of the second ordinary silicon substrate in the embodiment;

[0020] Figure 2(b) shows a schematic diagram of the structure of silicon substrate B1 in the embodiment;

[0021] Figure 2(c) shows a schematic diagram of the structure of silicon substrate B2 in the embodiment;

[0022] Figure 2(d) shows a schematic diagram of the structure of silicon substrate B3 in the embodiment;

[0023] Figure 2(e) shows a schematic diagram of the support layer in the embodiment;

[0024] Figure 3 The diagram shown illustrates the bonding of the support layer, epoxy resin, and device layer in this embodiment.

[0025] Figure 4 The diagram shown is a schematic of etching the bonding structure of the support layer, epoxy resin and device layer in the embodiment.

[0026] Figure 5 The image shown is a cross-sectional view of the finished product obtained by the method of fabricating micromechanical suspended structures using ordinary silicon substrates in the embodiment.

[0027] Figure 6 The image shown is a top view of the finished product obtained by the method of fabricating micromechanical suspended structures using a common silicon substrate in the embodiment. Detailed Implementation

[0028] To further illustrate the various embodiments, the present invention provides accompanying drawings. These drawings are part of the disclosure of the present invention, primarily used to illustrate the embodiments and to explain the operating principles of the embodiments in conjunction with the relevant descriptions in the specification. With reference to these drawings, those skilled in the art should be able to understand other possible implementations and the advantages of the present invention. Components in the drawings are not drawn to scale, and similar component symbols are generally used to represent similar components.

[0029] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments.

[0030] This embodiment provides a method for fabricating micromechanical suspended structures using ordinary silicon substrates. Specifically, ordinary silicon substrates refer to single-layer silicon wafers, which can be understood as silicon wafer structures directly cut from silicon ingots.

[0031] The method for fabricating micromechanical suspended structures using ordinary silicon substrates includes the following steps:

[0032] S1, refer to Figures 1(a) to 1(d) As shown, a first ordinary silicon substrate 10 is selected, and multiple micromechanical suspended structures are obtained on the first ordinary silicon substrate 10 through incomplete etching. The multiple micromechanical suspended structures constitute the device layer 11 and are connected by an incompletely etched bottom connection layer 12. Each micromechanical suspended structure includes a fixed area and a cantilever structure connecting the fixed area.

[0033] like Figure 6 As shown in this specific embodiment, there are three micromechanical suspension structures. The fixed areas (1, 2, 3) of the three micromechanical suspension structures are isolated from each other and form a quadrilateral frame. Cantilever 7 connects to fixed area 1, cantilever 8 connects to fixed area 2, and cantilever 9 connects to fixed area 3. The cantilever structures of the three micromechanical suspension structures extend to the center.

[0034] S2, refer to Figures 2(a) to 2(e) As shown, a second ordinary silicon substrate 20 covered with silicon nitride films (21, 22) on both sides is selected, and the support layer 4 is obtained by complete etching.

[0035] Specifically, the support layer 4 is a hollow quadrilateral frame structure, which corresponds to the quadrilateral frame formed by the fixed areas (1, 2, 3) of the three micromechanical suspended structures in the first ordinary silicon substrate 10.

[0036] S3, as Figure 3 As shown, the support layer 4 obtained in step A2 and the device layer 11 obtained in step S1 are bonded together, so that the support layer 4 simultaneously fixes the fixing areas (1, 2, 3) of multiple micromechanical suspended structures; the cantilever (7, 8, 9) are not connected to the support layer 4.

[0037] S4, as Figure 4 As shown, the bottom interconnect layer 12 of the first ordinary silicon substrate 10 is completely etched to separate multiple micromechanical suspended structures, thus obtaining the micromechanical suspended structure.

[0038] Thus, the final result is as follows Figure 5 and Figure 6 The finished product shown has three fixed areas (1, 2, 3) of the micromechanical suspended structure supported and connected by the support layer 4, while the cantilever (7, 8, 9) is suspended. That is, the device layer 11 of the product is prepared by the first ordinary silicon substrate 10, the bonding layer between the first ordinary silicon substrate 10 and the second ordinary silicon substrate 20 serves as an insulating layer, and the support layer 4 of the product is prepared by the second ordinary silicon substrate 20.

[0039] This scheme designs a method for fabricating micromechanical suspended structures using ordinary silicon substrates, enabling the use of ordinary silicon substrates instead of SOI silicon wafers for fabricating micromechanical suspended structures. This effectively solves the problems of high material and processing costs, as well as the difficulty in releasing the SiO2 layer, encountered when using SOI silicon wafers for fabrication. It features low cost, relatively simple fabrication, and low difficulty.

[0040] Specifically, in this embodiment, step S1 includes the following: S11, as shown in Figures 1(a) and 1(b), a patterned protective layer 31 with a micromechanical suspended structure is prepared on the front side of the first ordinary silicon substrate 10. Specifically, the patterned protective layer 31 is prepared by using a photoresist mask to obtain the silicon substrate A1 shown in Figure 1(b).

[0041] S12, perform deep silicon etching on the front side of silicon substrate A1, without etching through the back side of silicon substrate A1, to obtain silicon substrate A2 as shown in Figure 1(c).

[0042] Thus, the etched upper layer becomes a micromechanical suspended structure, namely device layer 11, while the unetched lower layer forms a bottom connection layer 12 that supports and connects the micromechanical suspended structure.

[0043] Specifically, in this step, during deep silicon etching, the bottom of the etched area with a wider trench generally reaches the bottom of the silicon substrate first than the bottom of the etched area with a narrower trench. Etching stops when the trench depth formed by the widest etched area reaches 50%-80% of the total thickness of the first ordinary silicon substrate 10, thus ensuring that the back side of the first ordinary silicon substrate 10 is not penetrated; it also ensures that the bottom bonding layer 12 has sufficient thickness for support. Specifically, the trench depth of the etched area is measured using a profilometer, which can be implemented using testing equipment such as a profilometer.

[0044] S13, remove the patterned protective layer on the front side to obtain silicon substrate A3 as shown in Figure 1(d). Specifically, rinse with ethanol and deionized water and then blow dry.

[0045] In this way, multiple micromechanical suspended structures are obtained on the first ordinary silicon substrate 10 through incomplete etching.

[0046] Specifically, in this embodiment, step S2 includes the following:

[0047] S21, silicon nitride films (21, 22) are coated on both sides of the second ordinary silicon substrate 20 as shown in Figure 2(a) to obtain silicon substrate B1 as shown in Figure 2(b); specifically, silicon nitride films can be coated on both sides of the second ordinary silicon substrate 20 by LPCVD (low pressure chemical vapor deposition) to achieve good uniformity.

[0048] S22, a photoresist mask 32 with a support layer pattern is prepared on the front side of silicon substrate B1 to obtain silicon substrate B2 as shown in Figure 2(c);

[0049] S23, the silicon nitride film 21 exposed on the front side of the silicon substrate B2 outside the photoresist mask 32 is etched away, and then the photoresist mask 32 is removed to obtain the silicon substrate B3.

[0050] Furthermore, the specific method of this step is as follows: the front side of the silicon substrate B2 is etched using reactive ion etching or ion beam etching process to etch through the silicon nitride layer exposed outside the photoresist mask. After etching, it is soaked in acetone and rinsed with deionized water to remove the photoresist mask, thus obtaining the silicon substrate B3 as shown in Figure 2(d).

[0051] S24, the silicon substrate B3 is etched to remove the silicon base layer covered by the unnitride film 21, resulting in silicon substrate B4.

[0052] Furthermore, the specific method of this step is as follows: using a wet etching process, the silicon substrate B3 is placed in a KOH solution or a tetramethylammonium hydroxide solution to remove the silicon substrate of the portion of the silicon substrate B3 that is not covered by the silicon nitride film 21, and then cleaned to obtain the silicon substrate B4.

[0053] S25, a photoresist mask with a support layer pattern is prepared on the silicon nitride film 22 on the bottom surface of the silicon substrate B4 and etched to obtain the support layer 4 as shown in Figure 2(e).

[0054] Specifically, the method for preparing the photoresist mask in this step is the same as in step S22, and the method for etching the silicon nitride film 22 in this step is the same as in step S23. These will not be described again here.

[0055] Furthermore, in this embodiment, step S3 specifically includes the following:

[0056] S31, such as Figure 3 As shown, the support layer 4 obtained in S2 and the device layer 11 obtained in S1 are bonded together by a bonding process. For example, in this embodiment, epoxy resin is used as the bonding layer 40 to bond the support layer 4 and the device layer 11 together; thus, the bonding layer 40 also serves as an insulating layer, achieving further insulation.

[0057] S32, as Figure 4 As shown, the bottom interconnect layer 12 of the first ordinary silicon substrate 10 is completely etched upwards, that is, the bottom interconnect layer 12 of the first ordinary silicon substrate 10 is completely etched away, thereby releasing the device layer 4, and finally completing the fabrication, resulting in the following: Figure 5 and Figure 6 The product shown.

[0058] Specifically, such as Figure 6As shown,

[0059] Specifically, in this embodiment, the thickness of the first ordinary silicon substrate 10 and the second ordinary silicon substrate 20 is 50-500 μm (micrometers) to ensure sufficient thickness while keeping the overall thickness within a preset range.

[0060] Specifically, the cross-sectional SEM image of the silicon substrate A2 obtained in step S12 above is shown below. Figure 4 As shown, the grooves formed by the wider etching area are deeper than those formed by the narrower etching area, and the verticality and flatness of the sidewalls of the etching groove are higher.

[0061] The side view SEM image of the finished device obtained in step S32 is shown below. Figure 5 As shown, the etched area has been completely penetrated, releasing the suspended structure. The verticality and flatness of the sidewalls of the suspended structure are high. Testing revealed that adjacent suspended structures are insulated from each other, and the fixed structures on both sides are also insulated, i.e. Figure 6 The three fixed zones shown are mutually insulated.

[0062] The test results above show that the sidewalls of the main suspended structure are relatively flat and vertical, and good electrical insulation is achieved between different fixing structures. Therefore, the method of the present invention is simple and effective, and can be widely applied to the fabrication of MEMS suspended structures.

[0063] This invention uses ordinary silicon substrates instead of SOI silicon wafers to fabricate micromechanical suspended structures, which has the following advantages:

[0064] (1) Two ordinary silicon substrates are used instead of SOI silicon wafers, and the entire process only requires two photomasks, which can greatly reduce the process cost.

[0065] (2) The suspended structure prepared on the first ordinary silicon substrate can be etched using a single mask, and there is no alignment deviation problem of secondary photolithography for the suspended structure.

[0066] (3) During the release process of the suspended structure (i.e. step S32), the device does not need to come into contact with the solution, which can effectively avoid the adhesion problem between micro-mechanical suspended structures caused by the liquid environment.

[0067] (4) This method has a wide range of applications and is of great value for processing suspended structures such as arms, beams, springs, and comb teeth.

[0068] (5) For the micromechanical structure of capacitive sensors, in order to improve sensor sensitivity and reduce unnecessary stray capacitance, the first ordinary silicon substrate for fabricating the device layer and the second ordinary silicon substrate for fabricating the support layer can be processed using silicon wafers with low resistivity and high resistivity, respectively, which can effectively improve the accuracy of the sensor.

[0069] Although the invention has been specifically shown and described in conjunction with preferred embodiments, those skilled in the art should understand that various changes in form and detail may be made to the invention without departing from the spirit and scope of the invention as defined in the appended claims, all of which shall be within the scope of protection of the invention.

Claims

1. A method for fabricating micromechanical suspended structures using a common silicon substrate, characterized in that, Includes the following steps: S1. Select a first ordinary silicon substrate and obtain multiple micromechanical suspended structures on the first ordinary silicon substrate through incomplete etching. The multiple micromechanical suspended structures constitute a device layer and are connected by an incompletely etched bottom connection layer. Each micromechanical suspended structure includes a fixed area and a cantilever structure connecting the fixed area. S2, Select a second ordinary silicon substrate covered with silicon nitride films on both sides, and obtain the support layer by complete etching; S3, bond the support layer obtained in step A2 and the device layer obtained in step S1 together, so that the support layer simultaneously fixes the fixing area of ​​multiple micromechanical suspended structures. S4, completely etch the bottom interconnect layer of the first ordinary silicon substrate to separate multiple micromechanical suspended structures; thus obtaining the micromechanical suspended structure; Step S2 specifically includes the following: S21, silicon nitride films are coated on both sides of the second ordinary silicon substrate to obtain silicon substrate B1; S22, a photoresist mask with a support layer pattern is prepared on the front side of silicon substrate B1 to obtain silicon substrate B2; S23, the silicon nitride film exposed outside the photoresist mask on the front side of silicon substrate B2 is etched away, and then the photoresist mask is removed to obtain silicon substrate B3; S24, etch silicon substrate B3 to remove the silicon base layer without silicon nitride film coverage, to obtain silicon substrate B4; S25, a photoresist mask with a support layer pattern is prepared on the silicon nitride film on the bottom surface of silicon substrate B4, and then etched to obtain the support layer.

2. The method for fabricating micromechanical suspended structures using a common silicon substrate according to claim 1, characterized in that: Step S1 specifically includes the following: S11, a patterned protective layer with a micromechanical suspended structure is prepared on the front side of the first ordinary silicon substrate to obtain silicon substrate A1; S12, perform deep silicon etching on the front side of silicon substrate A1, without etching through the back side of silicon substrate A1, to obtain silicon substrate A2; S13, remove the patterned protective layer on the front side to obtain silicon substrate A3.

3. The method for fabricating micromechanical suspended structures using a common silicon substrate according to claim 2, characterized in that: In step S12, etching is stopped when the depth of the etched area with the widest groove reaches 50%-80% of the total thickness of the first ordinary silicon substrate.

4. The method for fabricating micromechanical suspended structures using a common silicon substrate according to claim 1, characterized in that: Step S24 is as follows: Using a wet etching process, the silicon substrate B3 is placed in a KOH solution or a tetramethylammonium hydroxide solution to remove the silicon substrate without silicon nitride coverage on the silicon substrate B3, and then rinsed clean.

5. The method for fabricating micromechanical suspended structures using a common silicon substrate according to claim 1, characterized in that: Step S3 specifically includes the following: S31, the support layer obtained in S2 and the device layer obtained in S1 are bonded together by a bonding process; S32, the bottom interconnect layer of the first ordinary silicon substrate is completely etched with the top facing up.

6. The method for fabricating micromechanical suspended structures using a common silicon substrate according to claim 1, characterized in that: The thickness of the first and second ordinary silicon substrates is 50-500 μm.

Citation Information

Patent Citations

  • A kind of method for preparing micromechanical suspended structure on soi silicon wafer

    CN104118845B

  • High depth-width ratio micro-machining based on silicon-silicon linking

    CN101244802A