A waste mud solidified cement soil-EPS particle material and a preparation method thereof

By preparing solidified cement-soil-EPS particle material from waste mud, the problem of reusing waste mud in bored pile construction has been solved, forming a lightweight building material and realizing environmentally friendly and efficient waste mud treatment and reuse.

CN117756499BActive Publication Date: 2026-11-20BEIJING UNIV OF TECH +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311852842.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2026-11-20
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively address the issue of reusing waste mud generated during bored pile construction, leading to environmental pollution and impacting construction progress.

Method used

By mixing wet mud, cement, auxiliary cementitious materials and EPS particles, and then sintering and cooling them, a lightweight sintered material with honeycomb pores is formed. The EPS particles are used to create pores to form dispersed pores, thus preparing waste mud solidified cement soil-EPS particle material.

Benefits of technology

This technology enables the efficient reuse of waste mud, forming a new type of lightweight building material that is lightweight, high-strength, and has excellent thermal insulation properties. It solves the environmental pollution problem and improves the reuse efficiency of waste mud.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117756499B_ABST
    Figure CN117756499B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of waste slurry solidified cement-soil EPS granular material and its preparation method, it is related to building material technical field.The material of the present application is obtained by mixing wet mud, cement, auxiliary cementitious material and EPS granule after solidification, sintering, cooling;The mass ratio of dry matter in wet mud, cement, auxiliary cementitious material and EPS granule is 1:0.02-0.05:0.01-0.02:0.0005-0.001;The wet mud used is obtained by flocculation-filtration from waste slurry, and the moisture content is not higher than 50%.The present application makes full use of construction waste, solves the problem of environmental pollution caused by construction waste slurry, improves the recycling efficiency of construction waste slurry, and at the same time, combined with the incorporation of EPS granule and its sintering preparation process, a new type of lightweight building material with light weight, high strength and excellent thermal insulation performance can be formed, which has good market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, and in particular to a waste mud solidified cement soil-EPS particle material and its preparation method. Background Technology

[0002] With the vigorous development of national infrastructure, various building structures and bridge structures have experienced unprecedented development. Among these, foundation treatment has always been a crucial aspect of structural construction, significantly impacting project costs and overall quality. Currently, bored piles are a commonly used foundation reinforcement method in engineering design due to their mature construction technology and high bearing capacity. However, during construction, the mixing of drill cuttings gradually deteriorates the mud properties, generating large amounts of waste mud that is difficult to directly discharge and reuse. This not only affects construction progress and the construction site environment but also easily causes secondary environmental pollution. Therefore, how to treat and utilize waste mud from bored piles in a low-cost, environmentally friendly manner has become a problem that needs to be solved in the engineering field.

[0003] Currently, the main methods for treating waste mud both domestically and internationally include natural drying, flocculant-based solid-liquid separation, chemical solidification, land cultivation, and mechanical dewatering. Although different waste mud treatment methods have been proposed, the problem of waste mud reuse has not been adequately solved. Summary of the Invention

[0004] The purpose of this invention is to provide a solidified cement-EPS particle material made from waste mud and its preparation method, so as to solve the problems existing in the prior art.

[0005] To achieve the above objectives, the present invention provides the following solution:

[0006] This invention provides a solidified cement-EPS particle sintered material made from waste mud, cement, auxiliary cementitious materials and EPS particles, which is obtained by mixing, solidifying, sintering and cooling.

[0007] The mass ratio of dry matter, cement, auxiliary cementitious materials and EPS particles in the wet mud is 1:0.02-0.05:0.01-0.02:0.0005-0.001;

[0008] Furthermore, the wet mud is obtained by flocculation of waste mud slurry, and the moisture content is not higher than 50%; the EPS particles have a particle size of 2-4 mm.

[0009] Furthermore, the auxiliary cementing material includes fly ash, silica fume, mineral powder, or lime.

[0010] Furthermore, the sintering temperature is 1150-1200℃, preferably 1200℃; the sintering time is 1.5-2h, preferably 1.5h.

[0011] Furthermore, the cooling rate is ≤20℃ / min; the temperature after cooling is room temperature.

[0012] The waste mud used in this invention is waste mud from the construction of cast-in-place piles.

[0013] This invention also provides a method for preparing the above-mentioned waste mud solidified cement soil-EPS particle sintering material, comprising the following steps:

[0014] The wet mud, cement, auxiliary cementitious materials and EPS particles are mixed in a certain proportion, then cured and shaped to form a green embryo. After drying, preheating, sintering and cooling, the waste mud solidified cement soil-EPS particle sintered material is obtained.

[0015] Furthermore, the drying temperature is 500°C, and the drying time is preferably 2 hours; the preheating temperature is 800°C, and the preheating time is preferably 1 hour.

[0016] Furthermore, the sintering temperature is 1150-1200℃, preferably 1200℃, and the time is 1.5-2h, preferably 1.5h; the cooling rate is ≤20℃ / min; and the temperature after cooling is room temperature.

[0017] After sintering, EPS particles form a molten material, thereby creating dispersed pores inside the material, ultimately forming a lightweight sintered material with a honeycomb-like internal structure.

[0018] More specifically, by flocculating and filtering the waste mud, and controlling the mass ratio of the resulting wet mud to cement, auxiliary cementitious materials and EPS particles, waste mud solidified cement-EPS particle sintered materials with different strength indicators can be obtained.

[0019] This invention also provides the application of the above-mentioned waste mud solidified cement soil-EPS particle sintering material in the construction field.

[0020] Furthermore, the waste mud solidified cement-EPS particle sintered material is used as a wall panel in the construction field. More preferably, the waste mud solidified cement-EPS particle sintered material of the present invention can be used as a lightweight wall panel for building infill walls or partition walls.

[0021] This invention utilizes EPS particles to create pores within the material, reducing its mass by approximately 40% compared to solid wall panels. The sintered strength reaches that of ordinary sintered bricks. Furthermore, the presence of pores creates thermal breaks within the wall panel, hindering heat transfer. Testing shows that the thermal conductivity of this waste mud-solidified cement-EPS particle sintered material reaches 0.3-0.4 W / (m·K), approximately half that of ordinary sintered clay bricks.

[0022] The present invention discloses the following technical effects:

[0023] This invention makes full use of construction waste, solves the problem of environmental pollution from construction waste mud, and improves the reuse efficiency of construction waste mud. At the same time, by combining EPS particles with its sintering preparation process, a new type of lightweight building material with light weight, high strength and excellent thermal insulation performance can be formed. This material can be widely used in infill walls and interior partition walls in various buildings and has good market application prospects. Attached Figure Description

[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 This is a flow chart of the preparation process of the waste mud solidified cement soil-EPS particle sintering material of the present invention;

[0026] Figure 2 This is a photograph of the wet mud obtained by flocculation and filtration of waste mud in Example 1 of the present invention.

[0027] Figure 3 The image shows a physical picture of the cement and auxiliary cementitious materials of the present invention, wherein a is cement, b is silica fume, c is mineral powder, d is lime, and e is fly ash.

[0028] Figure 4 This is a photograph of the EPS particles used in this invention.

[0029] Figure 5 The image shows the actual preform of the waste mud solidified cement soil-EPS particle wall panel before sintering in Embodiment 1 of the present invention; a is the front view, and b is the side view.

[0030] Figure 6 This is a physical image of the waste mud solidified cement soil-EPS particle sintered wall panel of Embodiment 1 of the present invention. Detailed Implementation

[0031] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0032] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0033] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0034] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0035] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0036] Example 1

[0037] A lightweight wall panel made from solidified cement-EPS particles from waste mud, the raw material of which includes wet mud after flocculation and filtration treatment (… Figure 2 ), cement and its auxiliary cementitious materials ( Figure 3 ) and EPS particles ( Figure 4 ).

[0038] Step 1: Flocculate and filter the waste mud, design the mix ratio of solidified cement-soil EPS particle wall panels, and determine the proportion of each component of the wall panels, including flocculated and filtered wet mud, cement, silica fume and mineral powder and other auxiliary cementing materials and EPS particles. The moisture content of the wet mud should not exceed 50%.

[0039] Step Two: Based on the component proportions from Step One, determine the feeding sequence, optimal mixing time, and curing time for each component during the mixing and molding process. The feeding sequence is as follows: flocculated and filtered wet mud, cement and its auxiliary cementitious materials, and finally EPS particles. The mixing times for each component in the feeding sequence are 2 minutes, 3 minutes, and 2 minutes, respectively. The material is then molded in a mold and allowed to cure naturally. The molding process for waste mud solidified cement-EPS particle wall panels is as follows... Figure 5 (Proportion of item 11 in Table 1).

[0040] Step 3: The preform prepared in Step 2 is placed in a muffle furnace and subjected to a series of stages: high-temperature drying, preheating, sintering, and cooling. The high-temperature drying temperature is 500℃ for 2 hours; the preheating temperature is 800℃ for 1 hour; the sintering temperature is 1200℃ for 1.5 hours; and the cooling rate is 10℃ / min. The wall panel preparation is complete when the temperature drops to room temperature. Waste mud solidified cement soil-EPS particle sintered wall panel is shown below. Figure 6 As shown in Table 1, No. 11 mix proportion, the average compressive strength of the sintered wall panel was 5.0 MPa after testing.

[0041] Based on Example 1, this invention designed a strength test for sintered wall panels made from waste mud solidified cement soil-EPS particles with different component contents. The test mainly focused on the compressive strength of untreated waste mud solidified cement soil-EPS particle test blocks and sintered waste mud solidified cement soil-EPS particle wall panels. The test block size was 50mm*50mm*50mm, and the wall panel size was 50mm*80mm*30mm.

[0042] Table 1. Test results of strength of cement-EPS particle wall panels solidified from waste mud with different cementitious materials.

[0043]

[0044]

[0045] Note: The contents of cement, fly ash, lime, mineral powder, silica fume, and EPS particles in the table are all percentages of the dry matter mass in the corresponding wet mud.

[0046] According to the results in Table 1, the strength of cement-EPS particle specimens solidified from waste mud showed an upward trend with the increase of cement content and auxiliary cementitious materials. Among the auxiliary cementitious materials, fly ash had a more significant effect on improving the strength of cement-EPS particles than lime. In the mixed auxiliary cementitious materials, the combination of fly ash and silica fume could obtain higher compressive strength of the specimens.

[0047] Numbers 4, 16, and 17 are comparative groups designed to study different EPS particle contents. Number 16 has a small amount of EPS particles and fewer pores in the wall panel, but the strength of the sintered wall panel of number 16 is not improved compared to number 4. Number 17 has 0.15% EPS particles in the wall panel, and too many pores in the wall panel, resulting in a significant decrease in strength. Therefore, an EPS particle content of 0.1% is the optimal value.

[0048] Based on Example 1 (fly ash content 1.0%, mineral powder content 1.0%), the effects of different sintering temperatures and sintering times on the strength of the wall panel were studied to obtain the optimal sintering temperature and sintering time.

[0049] Table 2. Record of Strength Test Results of Waste Slurry Solidified Cement-EPS Particle Wall Panels under Different Sintering Schemes

[0050]

[0051] This invention addresses the problem of insufficient solidification and reuse of existing engineering waste mud by providing a lightweight wall panel made of solidified cement-soil-EPS particles. By processing waste mud, it prepares a new type of recyclable building material, thereby effectively improving the reuse efficiency of waste mud and solving the problems of difficult waste mud disposal and environmental pollution. It also provides a direction for the research and development of building materials.

[0052] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A sintered material made from solidified waste mud cement soil-EPS particles, characterized in that, It is obtained by mixing wet mud, cement, auxiliary cementitious materials and EPS particles, then curing, sintering and cooling. The contents of the cement, auxiliary cementitious materials, and EPS particles relative to the dry matter mass in the wet mud are as follows: When the cement content is 3.5%, the auxiliary cementitious material is fly ash, the fly ash content is 1.5%, and the EPS particle content is 0.1%. When the cement content is 3.0%, the auxiliary cementitious materials are fly ash and lime, the fly ash content is 1.0%, the lime content is 1.0%, and the EPS particle content is 0.1%. When the cement content is 3.0%, the auxiliary cementitious material is lime and mineral powder, the lime content is 1.0%, the mineral powder content is 1.0%, and the EPS particle content is 0.1%. When the cement content is 3.0%, the auxiliary cementitious materials are fly ash and silica fume, the fly ash content is 1.0%, the silica fume content is 1.0%, and the EPS particle content is 0.1%. The wet mud is obtained by flocculation of waste mud slurry, and its water content is not higher than 50%.

2. The waste mud solidified cement soil-EPS particle sintering material according to claim 1, characterized in that, The sintering temperature is 1150-1200℃, and the time is 1.5-2h.

3. The waste mud solidified cement soil-EPS particle sintering material according to claim 1, characterized in that, The cooling rate is ≤20℃ / min; the temperature after cooling is room temperature.

4. The preparation method of the waste mud solidified cement soil-EPS particle sintering material as described in claim 1, characterized in that, Includes the following steps: The wet mud, cement, auxiliary cementitious materials and EPS particles are mixed in a certain proportion, then cured and shaped to form a green embryo. After drying, preheating, sintering and cooling, the waste mud solidified cement soil-EPS particle sintered material is obtained.

5. The preparation method according to claim 4, characterized in that, The drying temperature is 500°C; the preheating temperature is 800°C.

6. The preparation method according to claim 4, characterized in that, The sintering temperature is 1150-1200℃, and the time is 1.5-2h; the cooling rate is ≤20℃ / min; and the temperature after cooling is room temperature.

7. The application of the waste mud solidified cement soil-EPS particle sintering material as described in any one of claims 1-3 in the construction field.

8. The application according to claim 7, characterized in that, The waste mud solidified cement soil-EPS particle sintered material is used as a wall panel.

Citation Information

Patent Citations

  • Production of water-holding granular sintered compact

    JP2000034179A