An epoxy curing agent for high solid graphene epoxy coating, a preparation method thereof and a graphene epoxy coating

By using acrylate and methacrylate-based aminopropyl POSS copolymerized to form POSS epoxy curing agent, the problem of low stereocrosslinking degree of epoxy coatings is solved, the strength and anti-corrosion performance of the coating are improved, the preparation process is simplified and the emission of organic compounds is reduced.

CN117757037BActive Publication Date: 2026-11-24ANHUI WILLY PAINT SCI & TECH LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311819774.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2026-11-24
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

The existing epoxy curing agents have a low degree of stereocrosslinking, resulting in insufficient strength and corrosion resistance of epoxy coatings, while also posing a problem of volatile organic compound emissions.

Method used

A high-solids graphene epoxy coating was prepared by copolymerizing acrylate and methacrylate-based aminopropyl POSS to form a POSS epoxy curing agent, which reacts with epoxy resin to form a three-dimensional cross-linked structure, thereby adjusting the hardness and reducing the viscosity.

Benefits of technology

It improves the heat resistance, strength, and corrosion resistance of epoxy coatings, reduces viscosity, simplifies the preparation process, and reduces the emission of organic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004633659570000121
    Figure BDA0004633659570000121
Patent Text Reader

Abstract

This invention relates to the field of graphene epoxy coating technology, and more particularly to a high-solids graphene epoxy coating epoxy curing agent, its preparation method, and the graphene epoxy coating itself. The epoxy curing agent is obtained by polymerizing acrylate and methacrylate-based aminopropyl POSS, with the methacrylate-based aminopropyl POSS comprising 20wt% to 60wt%. The high-solids graphene epoxy coating includes a main agent and additives, with a mass ratio of (1-2):(1.5-1), wherein the additives include the high-solids graphene epoxy coating epoxy curing agent described above. This invention, by introducing a POSS epoxy curing agent, achieves a hyperbranched structure and stereocrosslinking curing compared to conventional epoxy curing agents, thereby improving the curing effect. Applying the POSS epoxy curing agent to high-solids graphene epoxy coatings can improve their temperature resistance, strength, and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of graphene epoxy coating technology, and more particularly to an epoxy curing agent for high-solids graphene epoxy coating, its preparation method, and the graphene epoxy coating itself. Background Technology

[0002] Metal corrosion refers to the phenomenon where metal is damaged due to corrosion caused by the influence of the surrounding medium. While there are many methods for protecting metals, research and industrial practice from various countries have shown that applying organic coatings to metal surfaces is an effective, easy-to-implement, and economical method to prevent corrosion. High-solids coatings are environmentally friendly coatings evolved from traditional solvent-based coatings. National standards define high-solids coatings as those with a non-volatile volume fraction of 70% or more in the application state. The biggest advantage of high-solids coatings is that they significantly reduce VOC emissions, making them very environmentally friendly. Furthermore, existing equipment can be used during production and application without increasing investment. High-solids coatings represent an important direction for the development of solvent-free epoxy coating systems, offering significant environmental advantages.

[0003] Graphene epoxy coatings, as a novel coating material, possess excellent anti-corrosion and mechanical properties. Epoxy curing agents are an indispensable component in the curing process. Epoxy curing agents can combine with epoxy resins, enabling the coating to exhibit excellent corrosion resistance and mechanical properties after curing. Conventional epoxy curing agents are generally difunctional amines, which, when combined with difunctional epoxy resins, primarily exhibit linear or planar structures. For example, existing patent CN115093546B discloses a diamine-based epoxy curing agent and its preparation method, as well as a polyurethane anti-corrosion coating containing a diamine-based epoxy curing agent and its preparation method. This diamine-based epoxy curing agent, used together with epoxy resin, prepares a non-isocyanate polyurethane anti-corrosion coating with high substrate adhesion and anti-corrosion performance. However, on the one hand, the diamine epoxy curing agent combines with epoxy resin to form a linear or planar structure with a low degree of stereocrosslinking, resulting in less than ideal heat resistance, strength, and corrosion resistance of the coating; on the other hand, amine compounds pose a problem of volatile organic compound (VOC) emissions, which poses potential risks to the environment and human health; the preparation process of this diamine epoxy curing agent requires high-temperature reaction and is relatively complex. Summary of the Invention

[0004] In view of this, the present invention proposes an epoxy curing agent for high-solids graphene epoxy coatings, a method for preparing the same, and a graphene epoxy coating, to solve the problem that the low degree of stereocrosslinking of epoxy curing agents in the prior art leads to insufficient strength and corrosion resistance of epoxy coatings.

[0005] The technical solution of this invention is implemented as follows:

[0006] In a first aspect, the present invention provides an epoxy curing agent for a high-solids graphene epoxy coating, wherein the epoxy curing agent is obtained by polymerization of acrylate and methacrylate-aminopropyl POSS, and the proportion of methacrylate-aminopropyl POSS in the epoxy curing agent is 20wt% to 60wt%.

[0007] Specifically, a POSS epoxy curing agent is formed by copolymerizing acrylate and methacrylate-based aminopropyl POSS. Methacrylate-based aminopropyl POSS has a cage-like structure; after polymerization with acrylate, it reacts with the hydroxyl groups in the epoxy resin molecules to form a three-dimensional cross-linked structure, improving the performance of the epoxy resin and shortening the curing time. Simultaneously, by limiting the proportion of methacrylate-based aminopropyl POSS in the epoxy curing agent, the hardness and softness of the epoxy cured product can be further adjusted to achieve a balance between hardness and toughness, meeting the requirements for high hardness and high impact strength. Methacrylate-based aminopropyl POSS has a high viscosity; directly using it as a curing agent results in a high viscosity epoxy curing agent, which is detrimental to coating and flow. However, polymerization with acrylate can reduce the viscosity of the curing agent, improving its coating performance and flowability.

[0008] Furthermore, when the amount of methacrylate-based aminopropyl POSS added is 20% to 60%, the corresponding POSS proportion is 20% to 60%, the total molecular weight is 8500, each POSS epoxy curing agent contains 2 to 6 POSSes, each POSS contains 7 amino groups, that is, the amine value is 14 to 42 amino groups / 8500g, the amine value is 1.65 to 4.95 mmol / g, and the KOH is 92.4 to 277 mg / g.

[0009] Secondly, the present invention provides a method for preparing an epoxy curing agent for high-solids graphene epoxy coatings.

[0010] Includes the following steps:

[0011] S1. Mix methyl methacrylate, butyl acrylate, acrylic acid, AIBN and reaction solvent, and stir for 0.5 to 1.5 h to obtain a precursor solution;

[0012] S2. Mix methacrylate-based aminopropyl POSS, AIBN and reaction solvent and add to the precursor solution. Stir and react for 4-6 hours to obtain POSS epoxy curing agent.

[0013] Based on the above technical solutions, preferably, in step S1, the mass ratio of methyl methacrylate, butyl acrylate, acrylic acid and AIBN is 1:(0.3~0.35):0.005:(0.01~0.02), and the reaction solvent includes butyl acetate and xylene.

[0014] Further, in step S1, before preparing the precursor solution, the reaction solvent is refluxed at 80℃~90℃, and nitrogen gas is continuously introduced into the reaction solvent for 30 minutes to remove oxygen and moisture from the reaction solvent. The volume ratio of butyl acetate to xylene in the reaction solvent is 1:1. In step S1, AIBN acts as an initiator to initiate the polymerization reaction of methyl methacrylate, butyl acrylate, and acrylic acid to generate acrylate. In step S2, methacrylate-aminopropyl POSS and AIBN are added to the precursor solution. Under the initiation effect of AIBN, the acrylate and methacrylate-aminopropyl POSS polymerize to generate POSS epoxy curing agent.

[0015] Based on the above technical solutions, preferably, step S2 specifically includes:

[0016] S21. Mix methacrylate-aminopropyl POSS, AIBN and reaction solvent and add to the precursor solution, stir and react for 0.5 to 1.5 h;

[0017] S22. Add AIBN and the reaction solvent to the reaction system of step S21 and continue the reaction for 3.5 to 4.5 hours. After the reaction is completed, cool and remove the reaction solvent, add methanol, filter and purify, and vacuum dry to obtain POSS epoxy curing agent.

[0018] Based on the above technical solutions, preferably, in step S21, the amount of methacrylate-aminopropyl POSS added accounts for 20% to 60% of the total reaction mass, and the amount of AIBN added is 0.5% to 1.5% of the POSS mass; in step S22, the amount of AIBN added is 1.5‰ to 2.5‰ of the total reaction mass.

[0019] Specifically, in step S2, AIBN is added in batches to avoid the polymerization reaction being too fast due to adding AIBN all at once, which would result in uneven molecular weight of the product. Adding AIBN in batches for initiation can promote the continuous release of free radicals by AIBN throughout the reaction process, thereby promoting the polymerization reaction of the monomer. This can avoid the reaction being too fast or uneven, and ensure that the product has a good molecular weight distribution and ideal properties.

[0020] Based on the above technical solutions, preferably, the preparation method of the methacrylate-aminopropyl POSS in step S2 includes:

[0021] S201. γ-aminopropyltriethoxysilane, sodium hydroxide, and tetrahydrofuran are refluxed at 65–75 °C for 4–6 h, then cooled to 24–27 °C and reacted for another 13–17 h to obtain Na3O. 12 Si7(C3H8N)7;

[0022] S202, Na3O 12 Si7(C3H8N)7, triethylamine, and anhydrous tetrahydrofuran were mixed and propyltrichloromethacrylate was added under a nitrogen atmosphere. The mixture was reacted at 0°C for 3–5 h, and then the temperature was raised to 24–27°C and the reaction was continued for 18–22 h to obtain methacrylate-aminopropyl POSS.

[0023] Based on the above technical solutions, preferably, the molar ratio of γ-aminopropyltriethoxysilane to sodium hydroxide is (2-2.5):1, and the Na3O 12 The molar ratio of Si7(C3H8N)7, triethylamine and propyltrichloromethacrylate is 1:1:(1.1~1.3).

[0024] Specifically, in step S201, γ-aminopropyltriethoxysilane undergoes a hydrolysis-condensation reaction with sodium hydroxide to generate Na3O. 12 Si7(C3H8N)7; In step S202, methacrylate-aminopropyl POSS with a complete cage-like structure is synthesized by using propyltrichloromethacrylate as a capping reagent through a vertex-capping reaction.

[0025] Thirdly, the present invention provides a high-solids graphene epoxy coating, comprising a main agent and an auxiliary agent, wherein the mass ratio of the main agent to the auxiliary agent is (1-2):(1.5-1);

[0026] The main agent comprises the following components by weight: 45-55 parts epoxy resin, 5-15 parts reactive diluent, 5-15 parts epoxy diluent, 5-15 parts rust inhibitor, 10-20 parts feldspar powder, 0.3-0.8 parts graphene, 0.1-0.5 parts wetting agent, 3-4 parts dispersant, 0.1-0.3 parts defoamer, 0.05-0.15 parts fumed silica, and 0.3-0.5 parts polyamide wax;

[0027] The additives include an epoxy curing agent for a high-solids graphene epoxy coating as described above.

[0028] Specifically, in the main component, epoxy resin serves as the primary curing agent and plasticizer, providing the coating with hardness, abrasion resistance, and chemical resistance; reactive diluents are used to adjust the viscosity and flowability of the coating, promoting its application performance during construction; epoxy diluents are used to adjust the solids content of the coating, affecting its drying time and film gloss; the addition of rust inhibitors provides corrosion protection for metal substrates, extending the coating's service life; feldspar powder increases the coating's volume, improving its abrasion resistance and durability; graphene enhances the coating's electrical conductivity, thermal conductivity, and mechanical properties; wetting agents improve the adhesion and wetting properties between the coating and the substrate, making the coating easier to apply; dispersants ensure the coating's uniformity and stability; defoamers prevent the formation of bubbles during construction, improving the film's appearance quality; fumed silica increases the coating's scratch resistance and hardness; and polyamide wax improves the coating's abrasion resistance and chemical resistance.

[0029] The amino groups in aminopropyl methacrylate POSS can undergo ring-opening reactions with the epoxy groups in epoxy resin to form new carbon-nitrogen bonds, thereby firmly attaching the POSS molecule to the epoxy resin molecular chain. Therefore, the highly cross-linked network structure formed by aminopropyl methacrylate POSS and epoxy resin promotes closer intermolecular spacing in the epoxy resin, thus improving its corrosion resistance. Furthermore, the organosilicon groups in the POSS molecule can also enhance its temperature resistance and strength.

[0030] Based on the above technical solutions, preferably, the active diluent includes allyl glycidyl ether or dodecyl glycidyl ether, the rust inhibitor includes one or more of high-purity zinc phosphate, aluminum tripolyphosphate and ion-exchange rust inhibitor, the wetting agent includes polysiloxane, the dispersant includes BYK-163, the defoamer includes DF-280, and the epoxy diluent includes xylene and n-butanol.

[0031] Based on the above technical solutions, preferably, the additives further include an epoxy diluent, and the mass ratio of the epoxy curing agent to the epoxy diluent is (6.5-7.5):(2.5-3.5), wherein the epoxy diluent includes xylene and n-butanol.

[0032] The epoxy curing agent for high-solids graphene epoxy coatings of the present invention, its preparation method, and the high-solids graphene epoxy coatings thereof have the following advantages over the prior art:

[0033] (1) By polymerizing methacrylate-based aminopropyl POSS with a complete three-dimensional cage structure with acrylate to form POSS epoxy curing agent, compared with conventional epoxy curing agent, the hyperbranched structure and three-dimensional cross-linking curing of the curing agent are realized, thereby improving the curing effect.

[0034] (2) By applying POSS epoxy curing agent to high solids graphene epoxy coatings, methacrylate-based aminopropyl POSS and epoxy resin can form a highly cross-linked network structure, making the molecular spacing of epoxy resin more compact, thereby improving its temperature resistance and strength; at the same time, the organic groups in POSS molecules can form island-like structures in epoxy resin, effectively preventing the intrusion of external substances, improving the sealing and salt spray resistance of epoxy resin, thereby improving the strength and anti-corrosion performance of graphene epoxy coatings; (3) The addition of POSS can form a nanoscale island-ocean structure, making the polymer structure more compact. By adjusting the proportion of methacrylate-based aminopropyl POSS in the curing agent, the degree of cross-linking and hardness of the polymer can be effectively controlled, thereby improving the hardness performance of high solids graphene epoxy coatings.

[0035] (4) The preparation process of the curing agent provided by the present invention is simple, does not require a high temperature and high pressure environment, and is inexpensive. Detailed Implementation

[0036] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0037] Example 1

[0038] This embodiment provides an epoxy curing agent for a high-solids graphene epoxy coating and its preparation method, wherein the epoxy curing agent contains 40 wt% methacrylate-aminopropyl POSS.

[0039] The preparation method of POSS epoxy curing agent specifically includes the following steps:

[0040] S1. γ-aminopropyltriethoxysilane (50.9 g, 0.23 mol), distilled water (5.25 g, 0.29 mol), sodium hydroxide (3.95 g, 0.1 mol), and tetrahydrofuran (250 mL) were placed in a 500 mL three-necked flask equipped with a reflux condenser. The reaction system was stirred and refluxed at 70 °C for 5 h, then cooled to 25 °C and stirred for another 15 h. Most of the tetrahydrofuran and other volatiles were removed by rotary evaporation. The mixture was dried in a vacuum oven at 40 °C for 24 h to obtain compound Na3O. 12 Si7(C3H8N)7;

[0041] S2. Add Na3O to a 500mL three-necked flask. 12Si7(C3H8N)7 (7.6 g, 8.8 mmol), triethylamine (1.3 mL, 8.8 mmol), and 200 mL of anhydrous tetrahydrofuran were mixed in a flask immersed in an ice-water bath and stirred until homogeneous. The mixture was then purged with high-purity nitrogen for 1 h. Propyltrichloromethacrylate (95%, 2.91 g, 10.56 mmol) was added to 20 mL of dry tetrahydrofuran and then slowly added dropwise to the reactor using a dropping funnel. The reaction system was stirred at 0 °C for 4 h, and then cooled to room temperature. Continue stirring the reaction at 25℃ for 20 h; centrifuge to remove the salt (NaCl) generated during the reaction, and take the supernatant; first add 40 g of distilled water to the supernatant, then add 40 g of chloroform, shake thoroughly for 20 min, let stand for 20 min, and then separate the organic layer (upper layer); wash the organic layer with distilled water until neutral, dry with anhydrous magnesium sulfate, centrifuge, remove most of the solvent using a rotary evaporator, and vacuum dry at 40℃ for 24 h to obtain methacrylate-aminopropyl POSS;

[0042] S3. Using a 1:1 volume ratio of butyl acetate and xylene as the reaction solvent, add 15g of the reaction solvent to a 100mL four-necked flask equipped with a constant speed stirrer, a constant pressure titration funnel, a reflux condenser, and an N2 gas delivery tube. Stir until homogeneous, reflux in an 85℃ constant temperature oil bath, and purge with high-purity nitrogen for 30min. Add 4.4g of methyl methacrylate (MMA), 1.45g of butyl acrylate (BA), 0.02g of acrylic acid (AA), 1g of the reaction solvent, and 0.06g of AIBN dropwise to the reactor over 1h, and continue stirring for another 1h. Add methyl methacrylate... Acrylate-based aminopropyl POSS (8.77 g), an appropriate amount of AIBN (0.150 g), and a reaction solvent (43.85 g) were slowly and uniformly added dropwise to the reactor (the amount of POSS added accounted for 40% of the total mass of the reactants, the mass fraction of the POSS solution was 20%, and the AIBN was added all at once). After stirring for 5 hours, the reaction was stopped and cooled to 25°C. Most of the solvent in the reaction solution was removed using a rotary evaporator. Under strong stirring, the solution was added dropwise to more than 10 times its volume of cold methanol, centrifuged to precipitate, and filtered for purification. The final precipitate was vacuum dried at 40°C to constant weight to obtain the epoxy curing agent.

[0043] Example 2

[0044] This embodiment provides an epoxy curing agent for high-solids graphene epoxy coatings and its preparation method. The epoxy curing agent contains 40 wt% methacrylate-based aminopropyl POSS. The preparation method is the same as in Example 1, except that in step S3, 8.77 g of methacrylate-based aminopropyl POSS, an appropriate amount of AIBN (0.0877 g), and 43.85 g of reaction solvent (POSS accounts for 40% of the total reactant mass, the POSS solution mass fraction is 20%, and AIBN is added in batches, with the first addition being 1% of the POSS mass) are added slowly and uniformly to the reactor, and the reaction is continued with stirring for 1 hour. Then, 0.062 g of AIBN (2‰ of the total reactant mass) and 2 g of reaction solvent are added to the reactor, and the reaction is continued for 4 hours before stopping and cooling to 25°C.

[0045] Example 3

[0046] This embodiment provides an epoxy curing agent for high-solids graphene epoxy coatings and its preparation method. The epoxy curing agent contains 20 wt% methacrylate-aminopropyl POSS. The preparation method of the epoxy curing agent is the same as in Example 2, except that the amount of methacrylate-aminopropyl POSS added in step S3 is 4.39 g, and the amount of POSS added accounts for 20% of the total mass of the reactants.

[0047] Example 4

[0048] This embodiment provides an epoxy curing agent for high-solids graphene epoxy coatings and its preparation method. The epoxy curing agent contains 60 wt% methacrylate-aminopropyl POSS. The preparation method of the epoxy curing agent is the same as in Embodiment 2, except that the amount of methacrylate-aminopropyl POSS added in step S3 is 13.16 g, and the amount of POSS added accounts for 60% of the total mass of the reactant monomers.

[0049] Example 5

[0050] This embodiment provides an epoxy curing agent for a high-solids graphene epoxy coating and its preparation method, wherein the epoxy curing agent contains 20 wt% methacrylate-aminopropyl POSS.

[0051] The preparation method of POSS epoxy curing agent specifically includes the following steps:

[0052] S1. γ-aminopropyltriethoxysilane (44.26 g, 0.2 mol), distilled water (5.25 g, 0.29 mol), sodium hydroxide (3.95 g, 0.1 mol), and tetrahydrofuran (250 mL) were placed in a 500 mL three-necked flask equipped with a reflux condenser. The reaction system was stirred and refluxed at 65 °C for 4 h, then cooled to 25 °C and stirred for another 13 h. Most of the tetrahydrofuran and other volatiles were removed by rotary evaporation. The mixture was dried in a vacuum oven at 40 °C for 24 h to obtain compound Na3O. 12 Si7(C3H8N)7;

[0053] S2. Add Na3O to a 500mL three-necked flask. 12 Si7(C3H8N)7 (7.6 g, 8.8 mmol), triethylamine (1.3 mL, 8.8 mmol), and 200 mL of anhydrous tetrahydrofuran were mixed in an ice-water bath and stirred until homogeneous. The mixture was then purged with high-purity nitrogen for 1 h. Propyltrichloromethacrylate (95%, 2.67 g, 9.68 mmol) was added to 20 mL of dry tetrahydrofuran and then slowly added dropwise to the reactor using a dropping funnel. The reaction system was stirred at 0 °C for 3 h, and then cooled to room temperature. Continue stirring the reaction at 25℃ for 18 hours; remove the salt (NaCl) generated during the reaction by centrifugation and take the supernatant; first add 40g of distilled water to the supernatant, then add 40g of chloroform, shake thoroughly for 20 minutes, let stand for 20 minutes, and then separate the organic layer (upper layer); wash the organic layer with distilled water until neutral, dry it with anhydrous magnesium sulfate, centrifuge, remove most of the solvent using a rotary evaporator, and vacuum dry at 40℃ for 24 hours to obtain methacrylate-aminopropyl POSS;

[0054] S3. Using a 1:1 volume ratio of butyl acetate and xylene as the reaction solvent, 15g of the reaction solvent was added to a 100mL four-necked flask equipped with a constant speed stirrer, a constant pressure titration funnel, a reflux condenser, and an N2 gas delivery tube. The mixture was stirred until homogeneous and then refluxed in an 85℃ constant temperature oil bath, purged with high-purity nitrogen for 30min. Methyl methacrylate (MMA) (4.4g), butyl acrylate (BA) (1.32g), acrylate (AA) (0.02g), the reaction solvent (1g), and AIBN (0.044g) were slowly and uniformly added to the reactor over 1h, and the reaction was continued with stirring for 0.5h. Methacrylate-based aminopropyl POSS (4.36g), an appropriate amount of AIBN (0.022g), and... The reaction solvent (21.8 g) (POSS accounts for 20% of the total reactant monomer mass, the POSS solution mass fraction is 20%, and AIBN is added in batches, with the first addition being 0.5% of the POSS mass) is added dropwise to the reactor at a uniform rate, and the reaction is continued to be stirred for 0.5 h. 1.5‰ of the total reactant monomer mass of AIBN (0.072 g) and 2 g of reaction solvent are added to the reactor, and the reaction is continued for 3.5 h before stopping and cooling to 25 °C. Most of the solvent in the reaction solution is removed using a rotary evaporator. Under strong stirring, the solution is added dropwise to more than 10 times its volume of cold methanol, centrifuged to precipitate, and filtered for purification. The final precipitate is vacuum dried at 40 °C to constant weight to obtain the epoxy curing agent.

[0055] Example 6

[0056] This embodiment provides an epoxy curing agent for a high-solids graphene epoxy coating and its preparation method, wherein the epoxy curing agent contains 60 wt% methacrylate-aminopropyl POSS.

[0057] The preparation method of POSS epoxy curing agent specifically includes the following steps:

[0058] S1. γ-aminopropyltriethoxysilane (55.33 g, 0.25 mol), distilled water (5.25 g, 0.29 mol), sodium hydroxide (3.95 g, 0.1 mol), and tetrahydrofuran (250 mL) were placed in a 500 mL three-necked flask equipped with a reflux condenser. The reaction system was stirred and refluxed at 75 °C for 6 h, then cooled to 25 °C and stirred for another 17 h. Most of the tetrahydrofuran and other volatiles were removed by rotary evaporation. The mixture was dried in a vacuum oven at 40 °C for 24 h to obtain compound Na3O. 12 Si7(C3H8N)7;

[0059] S2. Add Na3O to a 500mL three-necked flask. 12Si7(C3H8N)7 (7.6 g, 8.8 mmol), triethylamine (1.3 mL, 8.8 mmol), and 200 mL of anhydrous tetrahydrofuran were mixed in an ice-water bath in a flask with stirring. The mixture was then purged with high-purity nitrogen for 1 h. Propyltrichloromethacrylate (95%, 3.15 g, 11.44 mmol) was added to 20 mL of dry tetrahydrofuran and then slowly added dropwise to the reactor using a dropping funnel. The reaction system was stirred at 0 °C for 5 h, and then cooled to room temperature. Continue stirring the reaction at 25℃ for 22 h; remove the salt (NaCl) generated during the reaction by centrifugation and take the supernatant; first add 40 g of distilled water to the supernatant, then add 40 g of chloroform, shake thoroughly for 20 min, let stand for 20 min, and then separate the organic layer (upper layer); wash the organic layer with distilled water until neutral, dry it with anhydrous magnesium sulfate, centrifuge, remove most of the solvent using a rotary evaporator, and vacuum dry at 40℃ for 24 h to obtain methacrylate-aminopropyl POSS;

[0060] S3. Using a 1:1 mixture of butyl acetate and xylene as the reaction solvent, add 15g of the reaction solvent to a 100mL four-necked flask equipped with a constant speed stirrer, a constant pressure titration funnel, a reflux condenser, and an N2 gas delivery tube. Stir until homogeneous, reflux in an 85℃ oil bath, and purge with high-purity nitrogen for 30min. Add 4.4g of methyl methacrylate (MMA), 1.54g of butyl acrylate (BA), 0.02g of acrylic acid (AA), 1g of the reaction solvent, and 0.088g of AIBN dropwise to the reactor over 1h, and continue stirring for 1.5h. Add 13.23g of methacrylate-based aminopropyl POSS and an appropriate amount of AIBN (0.13g). The reaction solvent (66.15 g) (POSS accounts for 60% of the total reactant monomer mass, the POSS solution mass fraction is 20%, and AIBN is added in batches, with the first addition being 1% of the POSS mass) is added dropwise to the reactor at a uniform rate, and the reaction is stirred for 1.5 h. 0.2 g of AIBN (2‰ of the total reactant monomer mass) and 2 g of reaction solvent are added to the reactor, and the reaction is continued for 4.5 h before stopping and cooling to 25 °C. Most of the solvent in the reaction solution is removed using a rotary evaporator. Under strong stirring, the solution is added dropwise to more than 10 times its volume of cold methanol, centrifuged to precipitate, and filtered for purification. The final precipitate is vacuum dried at 40 °C to constant weight to obtain the epoxy curing agent.

[0061] Application Examples 1-6

[0062] This application example provides a high-solids graphene epoxy coating, comprising a main agent and additives in a mass ratio of 1.5:1. The main agent components include: 50g of E44 epoxy resin, 10g of allyl glycidyl ether, 10g of epoxy diluent (xylene / n-butanol = 7:3), 10g of high-purity zinc phosphate, 15g of feldspar powder, 0.5g of graphene, 0.3g of polysiloxane, 3.5g of BYK-163, 0.2g of DF-280, 0.1g of fumed silica, and 0.4g of polyamide wax. The additive components mainly include: 70g of epoxy curing agent and 30g of epoxy diluent (xylene / n-butanol = 7:3). The epoxy curing agent was prepared according to Examples 1 to 6.

[0063] Application Example 7

[0064] This application example provides a high-solids graphene epoxy coating with the same composition as application example 3, except that the mass ratio of the main agent to the additive is 1:1.5.

[0065] Application Example 8

[0066] This application example provides a high-solids graphene epoxy coating with the same composition as application example 4, except that the mass ratio of the main agent to the additive is 2:1.

[0067] Application Example 9

[0068] This application example provides a high-solids graphene epoxy coating with the same composition as application example 2, except that the main component of the additives includes only 100g of epoxy curing agent.

[0069] Application Example 10

[0070] This application example provides a high-solids graphene epoxy coating with the same composition as application example 2, except that the main additives include 65g of epoxy curing agent and 35g of epoxy diluent (xylene / n-butanol = 7:3). The epoxy curing agent is prepared in example 2.

[0071] Application Example 11

[0072] This application example provides a high-solids graphene epoxy coating with the same composition as Application Example 2, except that the main additives include 75g of epoxy curing agent and 25g of epoxy diluent (xylene / n-butanol = 7:3). The epoxy curing agent was prepared in Example 2.

[0073] Application Example 12

[0074] This application example provides a high-solids graphene epoxy coating, comprising a main agent and additives in a mass ratio of 1.5:1. The main agent components include: 50g of E44 epoxy resin, 10g of allyl glycidyl ether, 10g of epoxy diluent (xylene / n-butanol = 7:3), 10g of high-purity zinc phosphate, 15g of feldspar powder, 0.5g of graphene, 0.3g of polysiloxane, 3.5g of BYK-163, 0.2g of DF-280, 0.1g of fumed silica, and 0.4g of polyamide wax. The main additive components include: 65g of epoxy curing agent and 35g of epoxy diluent (xylene / n-butanol = 7:3). The epoxy curing agent was prepared using the method described in Example 2.

[0075] Application Example 13

[0076] This application example provides a high-solids graphene epoxy coating, comprising a main agent and additives in a mass ratio of 1.5:1. The main agent components include: 50g of E44 epoxy resin, 10g of dodecyl glycidyl ether, 10g of epoxy diluent (xylene / n-butanol = 7:3), 10g of aluminum tripolyphosphate, 15g of feldspar powder, 0.5g of graphene, 0.3g of polysiloxane, 3.5g of BYK-163, 0.2g of DF-280, 0.1g of fumed silica, and 0.4g of polyamide wax. The main additive components include: 75g of epoxy curing agent and 25g of epoxy diluent (xylene / n-butanol = 7:3). The epoxy curing agent was prepared using the method described in Example 2.

[0077] Comparative Example 1

[0078] This comparative example provides a graphene epoxy coating with the same composition as Application Example 2, except that the curing agent is a diamine epoxy curing agent, which is prepared according to the method in patent CN115093546B.

[0079] Performance testing

[0080] The graphene epoxy coatings prepared for Examples 1-13 and Comparative Example 1 were subjected to performance testing after curing at room temperature for 7 days. The tested properties included hardness, adhesion, impact resistance, and smoke resistance. Adhesion was tested according to ISO 4624 or ASTM 4541 standards using an AT-A automatic pull-out tester. A sandblasted iron plate with a film thickness of 150 micrometers was used, and the coating was tested after 24 hours of natural drying. Salt spray resistance was tested according to GB / T 1771. Hardness was tested according to the His hardness test method (ASTM D3363). Impact resistance was tested according to ISO 6272. Adhesion was tested using the cross-cutting method (ASTM D3359). The test results are shown in Table 1.

[0081] Table 1

[0082]

[0083] As shown in Table 1, comparing Application Example 1 and Application Example 2, the graphene epoxy coating prepared in Application Example 2 exhibits superior performance compared to Application Example 1. This is likely because the batch addition of AIBN during the epoxy curing agent preparation process promotes monomer polymerization, improves the uniformity of epoxy curing agent molecules, and thus enhances the performance of the epoxy curing agent. Comparing Application Example 2 with Application Examples 3, 4, 7, and 8, the amount of methacrylate-based aminopropyl POSS added affects the performance of the epoxy curing agent; a higher addition amount results in more reaction sites, better crosslinking, and higher hardness, thereby influencing the performance of the graphene epoxy coating. Comparing Application Example 2 with Application Examples 5 and 6, changes in the epoxy curing agent preparation process parameters can affect its performance, thus impacting the performance of the graphene epoxy coating. Comparing Application Example 2 with Application Examples 9-13, the proportion of the epoxy curing agent in the additives also affects the performance of the graphene epoxy coating. Comparing Application Example 2 with Comparative Example 1, the POSS-based epoxy curing agent provided by this invention significantly improves the performance of the graphene epoxy coating.

[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An epoxy curing agent for a high-solids graphene epoxy coating, characterized in that: The epoxy curing agent is obtained by polymerizing acrylate and methacrylate-aminopropyl POSS. The methacrylate-aminopropyl POSS accounts for 20wt% to 60wt% of the epoxy curing agent. Each POSS epoxy curing agent contains 2 to 6 POSSes, and each POSS contains 7 amino groups.

2. The method for preparing the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 1, characterized in that: Includes the following steps: S1. Mix methyl methacrylate, butyl acrylate, acrylic acid, AIBN and reaction solvent, and stir for 0.5~1.5h to obtain a precursor solution; S2. Mix methacrylate-based aminopropyl POSS, AIBN and reaction solvent and add to the precursor solution. Stir and react for 4-6 hours to obtain POSS epoxy curing agent.

3. The method for preparing the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 2, characterized in that: In step S1, the mass ratio of methyl methacrylate, butyl acrylate, acrylic acid, and AIBN is 1:(0.3~0.35):0.005:(0.01~0.02), and the reaction solvent includes butyl acetate and xylene.

4. The method for preparing the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 2, characterized in that: Step S2 specifically includes: S21. Mix methacrylate-aminopropyl POSS, AIBN and reaction solvent and add to the precursor solution, stir and react for 0.5~1.5h; S22. Add AIBN and the reaction solvent to the reaction system of step S21 and continue the reaction for 3.5~4.5h. After the reaction is completed, cool and remove the reaction solvent, add methanol, filter and purify, and vacuum dry to obtain POSS epoxy curing agent.

5. The method for preparing the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 4, characterized in that: In step S21, the amount of methacrylate-aminopropyl POSS added accounts for 20% to 60% of the total reaction mass, and the amount of AIBN added is 0.5% to 1.5% of the POSS mass; in step S22, the amount of AIBN added is 1.5‰ to 2.5‰ of the total reaction mass.

6. The method for preparing the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 2, characterized in that: The preparation method of methacrylate-aminopropyl POSS in step S2 includes: S201. γ-aminopropyltriethoxysilane, sodium hydroxide, and tetrahydrofuran are refluxed at 65-75°C for 4-6 hours, then cooled to 24-27°C and reacted for another 13-17 hours to obtain Na3O. 12 Si7(C3H8N)7; S202, Na3O 12 Si7(C3H8N)7, triethylamine, and anhydrous tetrahydrofuran were mixed and propyltrichloromethacrylate was added under a nitrogen atmosphere. The mixture was reacted at 0°C for 3-5 hours, and then the temperature was raised to 24-27°C and the reaction was continued for 18-22 hours to obtain methacrylate-based aminopropyl POSS.

7. The method for preparing an epoxy curing agent for a high-solids graphene epoxy coating as described in claim 6, characterized in that: The molar ratio of γ-aminopropyltriethoxysilane to sodium hydroxide is (2~2.5):1, and the Na3O 12 The molar ratio of Si7(C3H8N)7, triethylamine and propyltrichloromethacrylate is 1:1:(1.1~1.3).

8. A high-solids graphene epoxy coating, characterized in that: It includes a main agent and an auxiliary agent, wherein the mass ratio of the main agent to the auxiliary agent is (1~2):(1.5~1); The main agent comprises the following components by weight: 45-55 parts epoxy resin, 5-15 parts reactive diluent, 5-15 parts epoxy diluent, 5-15 parts rust inhibitor, 10-20 parts feldspar powder, 0.3-0.8 parts graphene, 0.1-0.5 parts wetting agent, 3-4 parts dispersant, 0.1-0.3 parts defoamer, 0.05-0.15 parts fumed silica, and 0.3-0.5 parts polyamide wax; The additives include the epoxy curing agent for a high-solids graphene epoxy coating as described in claim 1.

9. The high-solids graphene epoxy coating as described in claim 8, characterized in that: The active diluent includes allyl glycidyl ether or dodecyl glycidyl ether, the rust inhibitor includes one or more of high-purity zinc phosphate, aluminum tripolyphosphate and ion-exchange rust inhibitor, the wetting agent includes polysiloxane, the dispersant includes BYK-163, the defoamer includes DF-280, and the epoxy diluent includes xylene and n-butanol.

10. The high-solids graphene epoxy coating as described in claim 8, characterized in that: The additives also include an epoxy diluent, and the mass ratio of the epoxy curing agent to the epoxy diluent is (6.5~7.5):(2.5~3.5). The epoxy diluent includes xylene and n-butanol.

Citation Information

Patent Citations

  • Epoxy functional group containing nano-reinforcer for hybrid polymer epoxy resin

    CN104356284A

  • POSS-based low-temperature epoxy curing agent and epoxy floor paint thereof

    CN107698740A