A eutectic flux for self-fluxed pellets and method of use thereof
By using eutectic flux to generate a eutectic liquid phase in pellets, the problem of high lime flux consumption during blast furnace ironmaking of acidic pellets was solved, which improved the strength and yield of pellets and reduced fuel consumption.
Patent Information
- Application Number
- CN202311711890.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-12-13
AI Technical Summary
In existing technologies, acidic pellets have problems such as high lime flux consumption, high slag volume, high fuel consumption, and low output in blast furnace ironmaking. In addition, self-fluxing pellets have high energy consumption, which limits their application.
The self-fluxing eutectic flux for pellets is used, which contains components such as CaO, Fe₂O₃, SiO₂, and rare earth elements. It is melted in a high-temperature electric arc furnace and reacts with solid oxides to generate a eutectic liquid phase, which binds the mineral powder particles, improves the basicity and strength of the pellets, and reduces the reduction expansion rate.
This has enabled the reduction of lime flux and slag consumption in blast furnaces, the improvement of pellet strength and output, the reduction of fuel consumption, and the fulfillment of blast furnace production needs.
Smart Images

Figure CN117758000B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of iron ore powder pelletizing technology, and relates to a eutectic flux for self-fluxing pellets and its application method. Background Technology
[0002] Iron pellets are one of the main raw materials for blast furnace ironmaking. They have advantages such as uniform particle size, high strength, suitability for long-distance transportation and storage, good iron grade, and good metallurgical properties, which are beneficial for improving the permeability of the charge column and reducing the coke ratio during smelting. In recent years, the proportion of iron pellets in blast furnace ironmaking raw materials has been increasing. According to the basicity of the pellets, they are generally divided into acidic pellets (basicity CaO / SiO2 < 0.6), self-fluxing pellets (flux-type pellets) (basicity CaO / SiO2 = 0.6~1.2), and magnesian pellets. Acidic pellets have high grade and good strength, and are easy to transport over long distances; at the same time, most sintering plants require acidic pellets to be used in conjunction with high-basicity sinter to meet the requirements of blast furnace smelting. Therefore, most countries in the world still mainly produce acidic pellets.
[0003] Pelletizing is a crucial step in the production of iron ore pellets, essentially a process of combining tiny, discrete iron ore particles into larger clumps. Adding a binder to the pelletizing material effectively improves its pelletizing properties and enhances the molecular bonding force between particles within the green pellets, thereby increasing the strength and thermal stability of the green pellets. Bentonite is commonly used as a binder for acidic iron ore pellets. The main components of bentonite are silicon dioxide and aluminum oxide, and its usage reaches 1.5%–3.5%. Statistics show that for every 1% increase in bentonite usage, the iron grade of the pellets decreases by 0.6%. Therefore, when using these pellets in blast furnaces, lime flux needs to be added to react with SiO2 and Al2O3 in a physicochemical manner, generating blast furnace slag with an alkalinity (CaO / SiO2) of 1.0–1.3, achieving slag-iron separation and desulfurization effects in blast furnace ironmaking. Thus, using acidic iron ore in blast furnaces increases lime flux usage, slag volume, fuel consumption, and reduces output. Currently, developing new binders that can replace bentonite is the main trend in pelletizing development. Later, by adding limestone powder to iron concentrate, people increased the basicity of pellets to the range of 0.6% to 1.2% to produce self-fluxing pellets. However, there are still many shortcomings such as high energy consumption, which limits the application of self-fluxing pellets. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a self-fusing eutectic flux for pelletizing ore. The eutectic flux is added before pelletizing and mixing. The added eutectic flux has a low melting point and melts rapidly at the green pellet roasting temperature. It undergoes a vigorous physicochemical reaction with the surrounding solid oxides to generate a eutectic liquid phase containing more components. As these eutectic liquid phases rapidly flow, diffuse, and cool and crystallize within the pellets, they bind the mineral powder particles together, thereby increasing the basicity of the pellets, the strength of the finished pellets, reducing the reduction expansion rate, and achieving low-temperature reduction pulverization.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a self-fusing eutectic flux for pelletized minerals, wherein the eutectic flux contains the following components in mass percentage: CaO 20%–50%, Fe2O3 10%–40%, SiO2 2%–30%, and rare earth elements 2%–20%.
[0006] The eutectic flux described in the present invention also contains the following components by mass percentage: Al2O3 2% to 30%.
[0007] The eutectic flux described in this invention also contains the following components by mass percentage: MgO 2% to 30%.
[0008] The eutectic flux described in this invention is prepared from iron ore, lime, dolomite, and rare earth raw materials through crushing, proportioning, mixing, melting, cooling, crystallization, and further crushing. The mixing and melting are carried out in a high-temperature electric arc furnace, with the furnace temperature controlled at 1500–1800°C. The resulting eutectic flux contains eutectic molecules such as calcium ferrite, calcium aluminate, and calcium silicate.
[0009] The particle size of the eutectic flux in the technical solution of this invention is 100 mesh to 200 mesh.
[0010] Secondly, the present invention provides a method for using a eutectic flux for self-fluxing pellets, comprising the following steps: mixing the eutectic flux for sintered ore with iron concentrate, drying it to obtain dry-based pelletizing raw materials and conveying them to a pelletizing pan, simultaneously spraying a composite binder onto the pelletizing pan during the pelletizing operation to obtain green pellets, and then roasting the green pellets to obtain self-fluxing pellets.
[0011] The amount of eutectic flux used in the technical solution of this invention accounts for 1% to 3% of the mass of iron concentrate.
[0012] The composite binder used in the technical solution of this invention accounts for 0.03% to 0.8% of the mass of the dry-based pelletizing raw material.
[0013] The composite binder described in the technical solution of this invention comprises the following components by mass percentage: sodium humate 5%–15%, guar gum 10%–15%, sodium silicate 20%–40%, cellulose 20%–40%, and pregelatinized starch 20%–40%.
[0014] The composite binder described in the technical solution of this invention comprises the following components by mass percentage: sodium humate 5%–15%, perlidone 10%–15%, sodium silicate 20%–40%, cellulose 20%–40%, and pregelatinized starch 15%–30%.
[0015] The composite adhesive in the technical solution of this invention is not limited to the above-mentioned components. Water glass, diatomaceous earth, quicklime, borate, fly ash, cement, and soap clay in inorganic adhesives, and carboxymethyl cellulose, polypropylene resin, lignosulfonate, and polyvinyl alcohol in organic adhesives can all be any component of the composite adhesive.
[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: In this invention, the eutectic flux is added before pelletizing and mixing, and the composite binder is added during the pelletizing process. The added eutectic flux has a low melting point and melts rapidly at the green pellet roasting temperature. It undergoes a vigorous physicochemical reaction with the surrounding solid oxides to generate a eutectic liquid phase containing more components. As these eutectic liquid phases rapidly flow, diffuse, and cool and crystallize within the pellets, they bind the mineral powder particles together, thereby increasing the basicity of the pellets, the strength of the finished pellets, reducing the reduction expansion rate, and achieving low-temperature reduction pulverization.
[0017] The eutectic flux of this invention replaces part of the sodium-based bentonite binder, thereby reducing the sodium load of the blast furnace and the fuel consumption of pellet roasting. It reduces the amount of blast furnace slag by about 35 kg per ton of pellets and can increase the output of the blast furnace by about 2% per ton of pellets. Attached Figure Description
[0018] Figure 1 The present invention provides a process flow for the production of self-fluxing pellets using the eutectic flux of this invention. Detailed Implementation
[0019] The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the test methods in the following embodiments are conventional methods.
[0020] Example 1 Taking iron concentrate as an example, sourced from Daixian County, Shanxi Province, its main components are: TFe 64.98%, SiO2 6.78%, CaO 0.86%, MgO 0.74%, Mn 0.068%, P 0.025%, S 0.183%, moisture 10.18%, and fineness 97.20%. Based on the components and contents of the iron concentrate, two eutectic fluxes and two composite binders were designed.
[0021] This embodiment uses 1 ton of eutectic flux as an example, requiring 400 kg of iron ore, 400 kg of lime, 180 kg of light-burned dolomite, and 20 kg of rare earth elements. The main components and contents of the iron ore are as follows: TFe 64.98%, SiO2 6.78%, CaO 0.86%, MgO 0.74%; the lime is produced in-house, with the main components and contents being: CaO 85.74%, SiO2 2.99%, MgO 1.86%; the rare earth elements (Re) are sourced from Baotou, Inner Mongolia, with the main components and contents being: Nd 93.0%; the light-burned dolomite has the following main components and contents: CaO 44.71%, SiO2 1.20%, MgO 32.04%.
[0022] The above raw materials are crushed to a particle size of 5mm-45mm. After mixing, the mixture is fed into an electric arc furnace, ignited by electric current, and melted for 6-8 hours. After cooling and crystallization, the mixture is crushed to obtain a eutectic flux of 100-200 mesh. The components and contents of eutectic flux 1 are as follows: CaO 38.32%, Fe2O3 39.02%, Al2O3 3.01%, SiO2 4.53%, rare earth 1.12%; the components and contents of eutectic flux 2 are as follows: CaO 40.39%, Fe2O3 38.48%, MgO 3.32%, SiO2 4.41%, rare earth 1.40%.
[0023] In this embodiment, composite binder 1 consists of: 8 kg sodium humate, 12 kg guar gum, 35 kg sodium silicate, 15 kg cellulose, and 30 kg pregelatinized starch; composite binder 2 consists of: 8 kg sodium humate, 12 kg perlidone, 35 kg sodium silicate, 25 kg cellulose, and 20 kg pregelatinized starch. All components of the above composite binders are commercially available products.
[0024] Reference Figure 1 The process flow diagram shown illustrates the process of mixing the two eutectic fluxes with iron concentrate, drying them to obtain dry-based pelletizing raw materials, and then conveying them to the pelletizing pan. During pelletizing, two composite binders are simultaneously sprayed onto the pelletizing pan to obtain green pellets. The green pellets are then roasted to obtain self-fluxing pellets. The addition of bentonite binder is used as a comparative example during pelletizing. The quality indicators of the green pellets are shown in Table 1.
[0025] Table 1. Components of the eutectic flux As shown in Table 1, when a eutectic flux is added before mixing and drying, and a composite binder is sprayed during the pelletizing process, the self-fluxing pellets produced have similar indicators as those produced using pure bentonite, such as the number of green pellets falling, compressive strength, and bursting temperature.
[0026] The green pellets numbered 1 to 5 were heated and roasted, and their compressive strength at 950℃ and 1250℃ was tested. According to the national standard for pellet testing, the drum strength, reduction expansion rate and low-temperature reduction index (RDI+3.15) at 500℃ of the standard sample and the example were tested. The test results are shown in Table 2 below.
[0027] Table 2 Detection Indicators for Pellet Ore As shown in Table 2, when a eutectic flux is added before mixing and drying, and a composite binder is sprayed during the pelletizing process to form pellets, the resulting self-fluxing pellets have compressive strength at 950℃, compressive strength at 1250℃, drum strength, reduction expansion rate, and low-temperature reduction pulverization index RDI (+3.15) at 500℃, which are comparable to those with added bentonite. This meets the requirements for blast furnace production, and the alkalinity also meets the alkalinity requirements for self-fluxing pellets.
[0028] Example 2 The five types of pellets prepared in Example 1 were smelted. Based on 1 ton of pellets, various indicators were calculated, and the results are shown in Table 3.
[0029] Table 3 Smelting Indicators serial number Slag volume, kg Energy consumption, kg Production, kg 1 71.75 23.94 568.25 2 2.32 0.77 637.68 3 3.09 1.03 636.91 4 3.87 1.29 636.13 5 4.64 1.55 635.36 In summary, the present invention adds eutectic flux before mixing and composite binder to the pelletizing plate, which can replace bentonite, increase the grade of pellets, and thus reduce the amount of lime flux and slag in the blast furnace, lower the coke ratio, and increase output.
[0030] The embodiments described above are merely preferred embodiments of the present invention and are only used to explain the present invention. They are not intended to limit the scope of the present invention. For those skilled in the art, other implementation methods can be easily made by substitution or modification based on the technical content disclosed in this specification. Therefore, all changes and improvements made on the principle of the present invention should be included within the scope of the patent application of the present invention.
Claims
1. A method for using a self-fluxing eutectic flux for pelletized minerals, characterized in that, Includes the following steps: The eutectic flux is mixed with iron concentrate and dried to obtain dry-based pelletizing raw material, which is then conveyed to the pelletizing pan. During the pelletizing process, a composite binder is sprayed onto the pelletizing pan to obtain green pellets. The green pellets are then roasted to obtain self-fluxing pellets. The eutectic flux contains the following components by mass percentage: CaO 20%~50%, Fe2O3 10%~40%, SiO2 2%~30%, and rare earth 1%~20%. The eutectic flux is prepared from iron ore, lime, dolomite, and rare earth raw materials through crushing, proportioning, mixing, melting, cooling, crystallization, and crushing. The mixing and melting are carried out in a high-temperature electric arc furnace, with the furnace temperature controlled at 1500~1800℃. The composite binder includes the following components: sodium humate, guar gum or perlidone, sodium silicate, cellulose, and pregelatinized starch.
2. The method of using a self-fluxing eutectic flux for pelletized minerals according to claim 1, characterized in that, The amount of the eutectic flux used accounts for 1% to 3% of the mass of the iron concentrate.
3. The method of using a self-fluxing eutectic flux for pelletized minerals according to claim 1, characterized in that, The eutectic flux also contains the following components by mass percentage: Al2O3 2%~30%.
4. The method of using a self-fluxing eutectic flux for pelletized minerals according to claim 1, characterized in that, The eutectic flux also contains the following components by mass percentage: MgO 2%~30%.
5. The method of using a self-fluxing eutectic flux for pelletized minerals according to claim 1, characterized in that, The particle size of the eutectic flux is 100-200 mesh.
6. The method of using a self-fluxing eutectic flux for pelletized minerals according to claim 1, characterized in that, The amount of the composite binder used is 0.03% to 0.8% of the mass of the dry-based pelletizing raw materials.
7. The method of using a self-fluxing eutectic flux for pelletizing minerals according to claim 1, characterized in that, The composite binder comprises the following components by weight percentage: sodium humate 5%~15%, guar gum 10%~15%, sodium silicate 20%~40%, cellulose 20%~40%, and pregelatinized starch 20%~40%.
8. The method of using a self-fluxing eutectic flux for pelletizing minerals according to claim 1, characterized in that, The composite binder comprises the following components by weight percentage: sodium humate 5%~15%, perlidone 10%~15%, sodium silicate 20%~40%, cellulose 20%~40%, and pregelatinized starch 15%~30%.
Citation Information
Patent Citations
Metallurgical auxiliary material fluxing agent and preparation method thereof
CN101748235A
Metallurgy one-step process recovery method for rare-earth-containing and / or niobium-containing slag
CN106755651A
Preparation method for self-fluxing composite pellet
WO2020087593A1