High-strength high-toughness fe-mn-al-v-c austenitic low-density steel and method for manufacturing same

By adding V to Fe-Mn-Al-C steel and performing solid solution and aging treatments, the precipitation of κ-carbides is controlled, and the dispersion of VC particles is promoted. This solves the problem that Fe-Mn-Al-C austenitic low-density steel is difficult to simultaneously possess high strength and high toughness, and prepares a high-strength and high-toughness steel that meets the requirements of vehicle lightweighting.

CN117758159BActive Publication Date: 2026-11-24BEIJING INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410012962.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2026-11-24
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

Existing Fe-Mn-Al-C austenitic low-density steels are difficult to simultaneously possess high strength and high toughness. Current research often sacrifices one property to obtain another when trying to improve the balance between strength and plasticity.

Method used

By adding an appropriate amount of V to Fe-Mn-Al-C steel and performing suitable solid solution and aging treatments, the precipitation of κ-carbides can be controlled, promoting the dispersion of nano-sized VC particles on the matrix, thereby playing a precipitation strengthening role and improving the strength and toughness of the steel.

Benefits of technology

High-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel with a yield strength ≥1150MPa, tensile strength ≥1350MPa, and impact energy KV2 ≥60J at -40℃ was prepared to meet the requirements of vehicle lightweighting and conform to the concept of energy conservation and emission reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004649988970000041
    Figure BDA0004649988970000041
  • Figure BDA0004649988970000051
    Figure BDA0004649988970000051
Patent Text Reader

Abstract

This invention relates to a high-strength, high-toughness austenitic low-density steel and its preparation method, belonging to the field of metallic materials technology. The steel's chemical composition by mass percentage is: C 1.0–1.6 wt%, Al 8–10 wt%, Mn 22–30 wt%, V 0.1–1.0 wt%, Nb ≤ 0.1 wt%, with the remainder being Fe and unavoidable impurities. This method adds a certain amount of V to Fe-Mn-Al-C steel. Through appropriate solution treatment and high-temperature aging, the precipitation of κ-carbides is suppressed, while nano-sized VC particles can disperse and precipitate in the matrix, providing good precipitation strengthening and hindering crack propagation under load, while simultaneously improving the steel's strength and toughness. The steel has a yield strength ≥ 1150 MPa, tensile strength ≥ 1350 MPa, Charpy impact energy (KV²) ≥ 60 J at -40℃, and a density of 6.6–6.9 g / cm³. 3 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, belonging to the field of metallic materials technology. Background Technology

[0002] With the increasing demand for equipment performance, Fe-Mn-Al-C austenitic low-density steels are attracting more and more attention due to their advantages of low density and high strength. Austenitic low-density steels have relatively low yield strength in the solid solution state. They are generally strengthened by aging treatment to induce the dispersion of (Fe,Mn)3AlC nanoscale κ-carbide precipitates in the matrix. However, the large-scale precipitation of κ-carbide can easily lead to a loss of toughness. To obtain excellent toughness, it is necessary to suppress the dispersion of κ-carbide precipitation, but this sacrifices strength. Therefore, it is difficult for Fe-Mn-Al-C austenitic low-density steels to simultaneously possess both high strength and high toughness.

[0003] In existing technologies, there has been considerable research on improving the strength-ductility balance of austenitic low-density steel, but research and results on simultaneously improving strength and toughness are rarely reported. Chinese patent application CN115572885A discloses a method for preparing high-toughness low-density steel, which involves the composite addition of multiple microalloying elements V, Nb, Mo, and Ti to form high number density and volume fraction of grain boundary MC-type carbides, ensuring significant fine grains under finishing rolling and solution treatment conditions. Although the impact energy at -40℃ KV2 ≥ 80J, its yield strength is low (≥ 650MPa), failing to achieve the effect of high strength and high toughness balance. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method. By adding a certain amount of V to Fe-Mn-Al-C steel and through appropriate solid solution treatment and high-temperature aging treatment, the precipitation of κ-carbides is suppressed, while nano-sized VC particles can be dispersed and precipitated on the matrix, playing a good precipitation strengthening role and hindering crack propagation under load, while improving the strength and toughness of the steel.

[0005] The objective of this invention is achieved through the following technical solution:

[0006] A method for preparing a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel, wherein the chemical composition and its mass percentage, based on the total mass of the steel as 100%, are as follows: C 1.0-1.6wt%, Al 8-10wt%, Mn 22-30wt%, V 0.1-1.0wt%, Nb≤0.1wt%, with the remainder being Fe and unavoidable impurities;

[0007] The method steps include:

[0008] (1) Solution treatment: The steel plates after casting and hot rolling are solution treated at 950-1100℃ for 1-3 hours, and then cooled to room temperature in water to obtain the solution-treated steel plates.

[0009] (2) Aging: The solution-treated steel plate is aged at 700-900℃ for 0.5-3 hours and then cooled in water to room temperature to obtain a high-strength and high-toughness Fe-Mn-Al-VC austenitic low-density steel.

[0010] Preferably, the mass fraction of C is 1.2 to 1.5 wt%.

[0011] Preferably, the mass fraction of V is 0.5–0.8 wt%.

[0012] Preferably, the chemical composition and its mass percentage, based on the total mass of the steel (100%), are as follows: C 1.2–1.5 wt%, Al 8–10 wt%, Mn 22–30 wt%, V 0.5–0.8 wt%, Nb ≤ 0.1 wt%, with the remainder being Fe and unavoidable impurities.

[0013] Preferably, in step (1), the cast and hot-rolled steel plate is prepared by the following method: weighing and selecting raw materials according to the mass percentage of chemical composition, vacuum melting and remelting the raw materials, then holding them at a temperature of 1200±50℃ for 2~15h for homogenization treatment, and finally hot rolling, with an initial rolling temperature of 1100~1150℃ and a final rolling temperature ≥950℃, and cooling to room temperature to obtain the cast and hot-rolled steel plate.

[0014] Preferably, during smelting, raw materials are weighed and selected according to the mass percentage of chemical composition, and vacuum melting is carried out: the raw materials are loaded into the furnace, and the vacuum degree is evacuated to <50Pa. After heating until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool, the material is refined at a vacuum degree <1Pa and a temperature of 1600-1700℃ for 0.5-2 hours. After sufficient deoxidation, alloying is carried out under argon protection, and then the material is poured and cooled under vacuum to obtain a steel ingot. Then, remelting is carried out: the steel ingot is placed in the furnace, protected by argon, with a pressure of 100-150Pa, and heated until completely melted. After holding at this temperature for 2-5 hours, the remelted steel ingot is obtained.

[0015] Preferably, in step (1), the solution temperature is 1000-1050℃ and the heat preservation time is 1-2h.

[0016] Preferably, in step (2), the aging temperature is 750-850℃ and the heat preservation time is 1-2h.

[0017] The high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel of the present invention is prepared by the above method.

[0018] Beneficial effects:

[0019] (1) The present invention discloses a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel with a yield strength ≥1150MPa, a tensile strength ≥1350MPa, a Charpy impact energy (KV2) ≥60J at -40℃, and a density of 6.7~6.9g / cm³. 3 This meets the lightweight requirements of vehicles and other transportation tools, and aligns with the development concept of energy conservation and emission reduction.

[0020] (2) The present invention discloses a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method. This method involves adding a certain amount of V to Fe-Mn-Al-C steel. Solution treatment is performed at 1000–1050℃ to completely dissolve the carbides in the matrix, forming a supersaturated solid solution. Too low a solution temperature leads to incomplete solution, while too high a temperature causes grain growth, affecting strength and plasticity. After solution treatment, aging is performed, with the aging temperature strictly controlled between 700 and 900℃. Temperatures below 700℃ induce κ-carbides to nucleate in the matrix, affecting toughness. Temperatures above 900℃ exceed the precipitation temperature range of VC particles, making it difficult for VC to nucleate and grow. Only aging at 700–900℃ allows nano-sized VC particles to disperse and precipitate on the matrix, providing good precipitation strengthening and hindering crack propagation under load, while simultaneously improving the strength and toughness of the steel.

[0021] (3) The composition design of this invention is based on the following:

[0022] The main role of carbon (C) is to participate in MC (M = V, Nb) carbide precipitation strengthening, thereby increasing the strength of steel. C is also an important solid solution strengthening element, promoting austenite formation and reducing density. While increasing C content can improve steel strength, excessively high C content can lead to a significant decrease in the steel's ductility, toughness, and weldability, as well as increased cold brittleness and aging sensitivity. Therefore, the C content in this invention is 1.0–1.6 wt%, more preferably 1.2%–1.5%.

[0023] Mn is an austenite stabilizing element, and its main function is to promote the austenitization of the matrix. Austenitic microstructure allows steel to maintain a high work hardening rate and improves plasticity; however, high Mn content can lead to the formation of brittle β-Mn phases, increasing the tendency for cracking during rapid heating and cooling. Conversely, excessively low Mn content can result in the formation of ferrite phases, reducing ductility. Therefore, the Mn content in this invention is 22%–30%.

[0024] The density of Al is 2.7 g / cm³. 3 Al is the main element for reducing the density of steel. Too low an Al content will not achieve the goal of reducing steel density and increasing specific strength, while too high an Al content will promote ferrite formation, reducing the plasticity and toughness of the steel. Therefore, the Al content in this invention is 8% to 10%.

[0025] Nb can combine with C atoms to form stable MC-type carbides, which nucleate and pin grains at grain boundaries during smelting and casting, refining the grains and effectively reducing the precipitation driving force of κ-carbides, thereby inhibiting their precipitation and growth. However, excessive Nb content can lead to coarsening of MC-type carbides and the formation of inclusions at grain boundaries, reducing the material's ductility and toughness. Therefore, the Nb content in this invention is ≤0.1%.

[0026] The addition of V promotes the precipitation of VC nanoparticles within the grains. However, excessive V content can lead to coarsening of VC particles, greatly reducing the strengthening effect and deteriorating plasticity and toughness. If the V content is too low, the VC-type carbides produced cannot be dispersed and precipitated in the matrix, resulting in an insignificant strengthening effect. Therefore, the V content of the present invention is 0.1 to 1.0 wt%, more preferably 0.5% to 0.8%. Detailed Implementation

[0027] The present invention will be further described in detail below with reference to specific embodiments.

[0028] Tensile testing equipment: Electronic universal testing machine, model INSTRON5985.

[0029] The sample fabrication and testing procedures were carried out in accordance with the national standard GB / T228-2002; tensile strength, yield strength, and elongation were all measured by tensile stress-strain curves obtained from tensile tests in accordance with GB / T228-2002. The impact toughness test adopted the standard Charpy V-notch sample.

[0030] According to the chemical composition range of a low-density ultra-high-strength steel of the present invention, five furnaces of 39 kg alloy ingots were prepared by vacuum induction melting.

[0031] Table 1 shows the chemical composition (wt%) of the low-density ultra-high-strength steel obtained in the embodiments of the present invention.

[0032] Table 1

[0033]

[0034]

[0035] Example 1

[0036] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0037] (1) Smelting: According to Table 1, 1 # The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 30 minutes for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 100Pa, electric heating is applied, and the input power is gradually increased to 84kW. This power is maintained for 5 hours to completely melt the steel ingot. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0038] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 2 hours, and then cooled to room temperature with the furnace.

[0039] (3) Hot rolling: The homogenized steel ingot is hot rolled at an initial rolling temperature of 1050℃ and a final forging temperature of >950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0040] (4) Solution treatment: The rolled plate is solution treated at 1050℃ for 1 hour to obtain the solution-treated steel plate.

[0041] (5) Aging: The steel plate is aged at 750℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0042] TEM test results of the low-density steel after solution treatment and aging show that VC nanoparticles are dispersed within the grains of the steel, with an average size of 12 nm, and no diffraction spots of κ carbides were observed.

[0043] Example 2

[0044] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0045] (1) Smelting: According to Table 1, section 2 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 0.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Then, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 120Pa, electric heating is applied, and the input power is gradually increased to 87.5kW until the steel ingot is completely melted. This power is maintained for 2h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0046] (2) Homogenization treatment: Keep at 1200℃ for 2 hours, and then cool to room temperature with the furnace.

[0047] (3) Hot rolling: The homogenized steel ingot is hot rolled at a starting temperature of 1050℃ and a final forging temperature of 950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0048] (4) Solution treatment: The rolled plate is solution treated at 1000℃ for 2 hours to obtain the solution-treated steel plate.

[0049] (5) Aging: The steel plate is aged at 850℃ for 1 hour and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0050] TEM test results of the low-density steel after solution treatment and aging show that VC nanoparticles are dispersed within the grains of the steel, with an average size of 12 nm, and no diffraction spots of κ carbides were observed.

[0051] Example 3

[0052] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0053] (1) Smelting: According to Table 1, 3 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1650℃ for 1.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 150Pa, electric heating is applied, and the input power is gradually increased to 86kW until the steel ingot is completely melted. This power is maintained for 3h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0054] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 2 hours, and then cooled to room temperature with the furnace.

[0055] (3) Hot rolling: The homogenized steel ingot is hot rolled at a starting temperature of 1050℃ and a final forging temperature of 950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0056] (4) Solution treatment: The rolled plate is solution treated at 1050℃ for 1 hour to obtain the solution-treated steel plate.

[0057] (5) Aging: The steel plate is aged at 825℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0058] TEM test results of the low-density steel after solution treatment and aging show that VC nanoparticles are dispersed within the grains of the steel, with an average size of 12 nm, and no diffraction spots of κ carbides were observed.

[0059] Example 4

[0060] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0061] (1) Smelting: According to Table 1, section 4 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 0.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 150Pa, electric heating is applied, and the input power is gradually increased to 87kW until the steel ingot is completely melted. This power is maintained for 4h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0062] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 2 hours, and then cooled to room temperature with the furnace.

[0063] (3) Hot rolling: The homogenized steel ingot is hot rolled at a starting temperature of 1050℃ and a final forging temperature of 950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0064] (4) Solution treatment: The rolled plate is solution treated at 1050℃ for 1 hour to obtain the solution-treated steel plate.

[0065] (5) Aging: The steel plate is aged at 810℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0066] TEM test results of the low-density steel after solution treatment and aging show that VC nanoparticles are dispersed within the grains of the steel, with an average size of 12 nm, and no diffraction spots of κ carbides were observed.

[0067] Example 5

[0068] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0069] (1) Smelting: According to Table 1, 5 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 0.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 150Pa, electric heating is applied, and the input power is gradually increased to 87kW until the steel ingot is completely melted. This power is maintained for 4h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0070] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 10 hours, and then cooled to room temperature with the furnace.

[0071] (3) Hot rolling: The homogenized steel ingot is hot rolled at an initial rolling temperature of 1050℃ and a final forging temperature of >950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0072] (4) Solution treatment: The rolled plate is solution treated at 1050℃ for 1 hour to obtain the solution-treated steel plate.

[0073] (5) Aging: The steel plate is aged at 830℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0074] TEM test results of the low-density steel after solution treatment and aging show that VC nanoparticles are dispersed within the grains of the steel, with an average size of 12 nm, and no diffraction spots of κ carbides were observed.

[0075] Comparative Example 1

[0076] A high-strength, high-toughness Fe-Mn-Al-C austenitic low-density steel and its preparation method, specifically including the following steps:

[0077] (1) Smelting: According to Table 1, 6 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 0.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 150Pa, electric heating is applied, and the input power is gradually increased to 87kW until the steel ingot is completely melted. This power is maintained for 4h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0078] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 15 hours, and then cooled to room temperature with the furnace.

[0079] (3) Hot rolling: The homogenized steel ingot is hot rolled at an initial rolling temperature of 1050℃ and a final forging temperature of >950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0080] (4) Solution treatment: The rolled plate is solution treated at 1050℃ for 1 hour to obtain the solution-treated steel plate.

[0081] (5) Aging: The steel plate is aged at 750℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0082] In this comparative example, no V was added, and the other contents and heat treatment process were the same as in Example 1. After solution treatment and high-temperature aging, no κ-carbide and semi-coherent VC nanoparticles were observed to precipitate in the matrix by TEM testing. Although the impact absorption energy (80J) was significantly improved, the strength was sacrificed, and the yield strength was reduced to 710MPa.

[0083] Comparative Example 2

[0084] A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel and its preparation method, specifically including the following steps:

[0085] (1) Smelting: According to Table 1, 7 #The raw materials for the ultra-high strength steel corresponding to the furnace are selected by weighing the chemical composition by mass percentage. First, vacuum melting is carried out: the raw materials are loaded into a vacuum induction furnace, and when the vacuum degree is evacuated to <50Pa, electric heating is applied, and the input power is gradually increased until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool. Then, the furnace is held at a vacuum degree of <1Pa and a temperature of 1700℃ for 0.5h for refining. After sufficient deoxidation, alloying is carried out under argon protection. Then, the ingot is poured and cooled under vacuum to obtain a steel ingot. Next, remelting is carried out: the steel ingot is placed in an electroslag furnace, argon protection is applied, the pressure is 150Pa, electric heating is applied, and the input power is gradually increased to 87kW until the steel ingot is completely melted. This power is maintained for 4h to allow the steel ingot to be completely melted. Finally, the ingot is cooled to obtain the remelted steel ingot.

[0086] (2) Homogenization treatment: The remelted steel ingots are loaded into the furnace at a temperature of 600℃, and kept at a temperature of 1200℃ for 2 hours, and then cooled to room temperature with the furnace.

[0087] (3) Hot rolling: The homogenized steel ingot is hot rolled at a starting temperature of 1050℃ and a final forging temperature of >950℃. It is then cooled to room temperature in air to obtain the rolled plate.

[0088] (4) Solution treatment: The rolled plate is solution treated at 1000℃ for 2 hours to obtain the solution-treated steel plate.

[0089] (5) Aging: The steel plate is aged at 550℃ for 2 hours and then cooled in water to room temperature to obtain a high-strength, high-toughness austenitic low-density steel.

[0090] Although V was added to this comparative example, its aging treatment temperature was low, making it difficult for the semi-coherent VC particles to nucleate and grow. TEM tests showed that only coarse κ-carbide particles (average size of 2-5 nm) were diffusely distributed in the matrix. Although the yield strength was significantly improved to over 400 MPa, the impact absorption energy was significantly reduced to 25 J.

[0091] The austenitic low-density steels prepared in the examples and comparative examples were wire-cut and ground into tensile specimens with a cross-sectional size of 2×1mm and an original gauge length L0 of 8mm. V-notch specimens were also machined into specimens with a length of 55mm and a cross-sectional size of 10×10mm. 2 The notch depth was ~2mm, and the test temperature was -40℃. Mechanical property tests were conducted, and the results are shown in Table 2. R p0.2 R represents the yield strength. m A represents tensile strength, and A represents elongation.

[0092] Table 2

[0093] Example Furnace number <![CDATA[σ 0.2 / MPa]]> <![CDATA[σ b / MPa]]> A / % KV2 / J <![CDATA[Density / (g / cm 3 )]]> 1 1# 1150 1360 40 102 6.6 2 2# 1180 1370 37 80 6.8 3 3# 1155 1354 41 106 6.7 4 4# 1210 1420 28 61 6.9 5 5# 1190 1320 36 75 6.8 Comparative Example 1 6# 710 1210 61 80 6.7 Comparative Example 2 7# 1120 1310 36 25 6.7

[0094] In summary, the invention includes, but is not limited to, the above embodiments. Any equivalent substitutions or partial improvements made under the spirit and principles of this invention shall be considered to be within the protection scope of this invention.

Claims

1. A method for preparing high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel, characterized in that: Based on the total mass of the steel (100%), the chemical composition and its mass percentage are as follows: C 1.0~1.6 wt%, Al 8~10 wt%, Mn 22~30 wt%, V 0.5~0.8 wt%, Nb≤0.1 wt%, with the remainder being Fe and unavoidable impurities; The method steps include: (1) The steel plates after casting and hot rolling are solution treated at 1000~1050℃ for 1~2h, and then cooled in water to room temperature to obtain the solution treated steel plates. (2) The solution-treated steel plate is subjected to aging treatment at a temperature of 750~850℃ for 1~2h, and then cooled in water to room temperature to obtain a high-strength and high-toughness Fe-Mn-Al-VC austenitic low-density steel. The high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel contains VC nanoparticles dispersed within its grains. The steel exhibits a yield strength ≥1150 MPa, tensile strength ≥1350 MPa, Charpy impact energy (KV²) ≥60 J at -40℃, and a density of 6.7~6.9 g / cm³. 3 .

2. The method for preparing high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel as described in claim 1, characterized in that: The mass fraction of C is 1.2~1.5 wt%.

3. The method for preparing a high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel as described in claim 1, characterized in that: In step (1), the cast and hot-rolled steel plates are prepared by the following method: raw materials are weighed and selected according to the chemical composition mass percentage, the raw materials are vacuum melted and remelted, then homogenized at a temperature of 1200±50℃ for 2~15h, and finally hot-rolled at an initial rolling temperature of 1100~1150℃ and a final rolling temperature of ≥950℃, and cooled to room temperature to obtain the cast and hot-rolled steel plates.

4. The method for preparing high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel as described in claim 3, characterized in that: During smelting, raw materials are weighed and selected according to the mass percentage of chemical composition, and vacuum melting is carried out: the raw materials are loaded into the furnace, and the vacuum degree is evacuated to <50Pa. After heating until the raw materials are completely melted and no bubbles overflow from the surface of the molten pool, the material is refined at a vacuum degree <1Pa and a temperature of 1600~1700℃ for 0.5~2h. After sufficient deoxidation, alloying is carried out under argon protection, and then the material is poured and cooled under vacuum to obtain steel ingots. Remelting is then carried out: the steel ingots are placed in the furnace, protected by argon, at a pressure of 100~150Pa, and heated until completely melted. The temperature is then held for 2~5h to obtain remelted steel ingots.

5. A high-strength, high-toughness Fe-Mn-Al-VC austenitic low-density steel, characterized in that: It is prepared by the method described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Manufacturing method of high-strength high-toughness plastic austenitic low-density steel

    CN115572885A

  • 1000MPa-stage non-magnetic stainless steel hot-rolled plate and manufacturing method

    CN107119241A

  • Short-process production method for low-density steel based on thin-strip continuous casting

    CN115216704A

  • Fe-Mn-Al-Ni-Mo-C high-strength austenite low-density steel and preparation method thereof