Mini-led and preparation method thereof

By adjusting the deposition parameters of the SiO₂ layer and optimizing the bonding process using an acidic activation solution, the problems of dim brightness and dead LEDs caused by insufficient adhesion in Mini-LED products were solved, achieving efficient epitaxial layer transfer and bonding, and improving product yield.

CN117766647BActive Publication Date: 2026-11-20JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410116732.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2026-11-20
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

In the existing technology, the dimming and dead LED problems caused by epitaxial layer delamination during the end-use of Mini-LED products are mainly due to insufficient adhesion of the SiO₂ adhesive layer and the transferred sapphire layer.

Method used

By adjusting the silane flow rate and chamber pressure during the deposition of the SiO₂ layer on the epitaxial wafer surface, reducing the power to increase the compressive stress of the SiO₂ layer, and using an acidic activation solution to increase the amount of hydroxyl bonds, combined with high-temperature bonding technology, the bonding process between sapphire and the SiO₂ layer is optimized.

Benefits of technology

It significantly improves the adhesion between sapphire and the epitaxial layer, increases the yield of epitaxial layer transfer to sapphire, avoids dim and dead light issues, and improves product reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117766647B_ABST
    Figure CN117766647B_ABST
Patent Text Reader

Abstract

The application provides a Mini-LED preparation method and a Mini-LED. The preparation method comprises the following steps: growing an epitaxial layer on a substrate to obtain an epitaxial wafer; depositing a SiO2 layer on the surface of a GaP layer; placing the epitaxial wafer and sapphire after polishing into an acidic activation solution for activation treatment, wherein the acidic activation solution is composed of H2SO4, H2O2 and H2O in a volume ratio of 7:3:1; bonding the epitaxial wafer and sapphire after the activation treatment, and removing the substrate to obtain the Mini-LED. The SiO2 layer is deposited by adjusting the silane flow, increasing the cavity pressure and reducing the power, the compressive stress of the SiO2 is improved, the adhesion between the SiO2 layer and the sapphire and the Gap layer is improved, the conventional alkali activation method is cancelled by optimizing the activation method, and more hydrogen bonds are attached to the surface of the sapphire and the SiO2 layer, so that the bonding effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of Mini-LED technology, and in particular to a Mini-LED and its preparation method. Background Technology

[0002] The development trend of LEDs has evolved from early indoor and outdoor displays to high-density, high-contrast small-pitch displays, and then to the commercialization of Mini flip-chip RGB products.

[0003] Red Mini LEDs require substrate transfer due to the light absorption of their GaAs substrates. This involves removing the original GaAs substrate and transferring the luminescent epitaxial layer onto a sapphire substrate for further fabrication of the Mini LED device. Current industry technology primarily involves epitaxial layer transfer through processes such as epitaxial wafer growth, phosphide cleaning before the bonding layer deposition line, GaP roughening, pre-deposition cleaning of the bonding layer, deposition, polishing, activation, bonding, and substrate removal.

[0004] In the current technology, the red light Mini products currently suffer from dimming and dead light problems due to epitaxial layer delamination during end-user use. This is mainly due to insufficient adhesion of the SiO2 adhesion layer and the transferred sapphire layer. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a Mini-LED and its preparation method, which solves the technical problem in the prior art where the adhesion of the SiO2 adhesive layer and the transferred sapphire layer is insufficient, leading to products that are prone to dim lighting and dead LEDs.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solution: a Mini-LED fabrication method, comprising the following steps: growing an epitaxial layer on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on a side away from the substrate; performing a first cleaning treatment on the epitaxial wafer and roughening the surface of the GaP layer; performing a second cleaning treatment on the roughened epitaxial wafer and depositing a SiO2 layer on the surface of the GaP layer; polishing the surface of the SiO2 layer and immersing the polished epitaxial wafer and sapphire in an acidic activation solution for activation treatment; bonding the activated epitaxial wafer and the sapphire and removing the substrate to obtain a Mini-LED.

[0007] According to one aspect of the above technical solution, the acidic activation solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 7:3:1.

[0008] According to one aspect of the above technical solution, the specific steps of bonding the activated epitaxial wafer and the sapphire crystal include:

[0009] Based on the first preset parameters, the activated epitaxial wafer and the sapphire are bonded at high temperature.

[0010] The first preset parameters include: bonding pressure of 8000 kgf-12000 kgf, bonding temperature of 400℃-500℃, and bonding time of 900 s-1000 s.

[0011] According to one aspect of the above technical solution, the step of depositing a SiO2 layer on the surface of the epitaxial wafer specifically includes:

[0012] An RF (radio frequency) technology is used, and a SiO2 layer is deposited on the surface of the epitaxial wafer based on a second preset parameter.

[0013] The second preset parameters include: radio frequency power of 90W-100W, pressure of 80Pa-100Pa, reaction gases of N2 and SiH4, and SiH4 flow rate of 290sccm-300sccm.

[0014] According to one aspect of the above technical solution, the step of sequentially cleaning the epitaxial wafer specifically includes:

[0015] The epitaxial wafer is immersed in the first cleaning solution and then rinsed clean with water.

[0016] The epitaxial wafer was immersed in a second cleaning solution and then rinsed clean with water.

[0017] The first cleaning solution is composed of H2O2, NH4OH, and H2O in a volume ratio of 2:1:1; the second cleaning solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 5:1:1.

[0018] According to one aspect of the above technical solution, the step of roughening the surface of the GaP layer specifically includes:

[0019] ICP etching technology is used to etch trenches on the surface of the GaP layer after a first cleaning process.

[0020] According to one aspect of the above technical solution, the steps for secondary cleaning of the roughened epitaxial wafer specifically include:

[0021] The epitaxial wafer was immersed in a third cleaning solution and then rinsed clean with water.

[0022] The third cleaning solution is composed of H₂SO₄, H₂O₂, and H₂O in a volume ratio of 5:1:1.

[0023] According to one aspect of the above technical solution, the step of removing the substrate to obtain a Mini-LED specifically includes:

[0024] A substrate etching solution is used to etch one side of the substrate of the bonded epitaxial wafer to remove the substrate and expose the epitaxial layer;

[0025] The surface of one side of the epitaxial layer of the epitaxial wafer is cleaned with acetone and isopropanol to obtain Mini-LED;

[0026] The substrate etching solution is composed of H2O2 and NH4OH in a volume ratio of 9:1.

[0027] According to one aspect of the above technical solution, the thickness of the SiO2 layer is...

[0028] On the other hand, the present invention also provides a Mini-LED, which is prepared by the Mini-LED preparation method described in the above technical solution.

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows: By using the above-mentioned second preset parameters to deposit and form a SiO2 layer, specifically by adjusting the silane flow rate, increasing the chamber pressure, and reducing the power, the compressive stress of SiO2 is improved, thereby improving the adhesion between the SiO2 layer and the sapphire and Gap layers. By optimizing the activation method and eliminating the conventional alkaline activation method, more hydrogen-oxygen bonds are attached to the surface of the sapphire and SiO2 layer, thereby improving the bonding effect. Furthermore, by using the above-mentioned first preset parameters to achieve the bonding of the sapphire and SiO2 layer, specifically by using a high-temperature bonding method, the adhesion between the sapphire and the epitaxial layer is further increased. Based on the above points, the yield of epitaxial layer transfer onto sapphire is greatly increased, avoiding the problems of dim brightness and dead light caused by epitaxial layer delamination during the end use of the product. Attached Figure Description

[0030] Figure 1 This is a flowchart of the Mini-LED fabrication method in the first embodiment of the present invention;

[0031] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation

[0032] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.

[0033] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.

[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0035] Example 1

[0036] Please see Figure 1 The figure shows a flowchart of the Mini-LED fabrication method in the first embodiment of the present invention, which includes the following steps:

[0037] Step S100: An epitaxial layer is grown on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on the side away from the substrate.

[0038] For ease of understanding, in some application scenarios of this embodiment, the substrate is a GaAs substrate, specifically using MOCVD technology, i.e., metal-organic chemical vapor deposition, to grow epitaxial layers on the substrate. MOCVD uses organic compounds of group III and group II elements and hydrides of group V and VI elements as crystal growth source materials, and performs vapor-phase epitaxy on the substrate through thermal decomposition reactions to grow thin single-crystal materials of various group III-V and group II-VI compound semiconductors and their multi-component solid solutions. Typically, crystal growth in MOCVD systems is carried out in a cold-walled quartz (stainless steel) reaction chamber under normal or low pressure (10-100 Torr) with H2 flowing through it. The substrate temperature is 500℃-1200℃, and a graphite substrate (with the substrate above it) is heated by DC. H2 carries the metal-organic compounds to the growth region through temperature-controlled liquid bubbling. The advantage of MOCVD technology is that it can precisely control the thickness, doping concentration, and composition of the epitaxial layer on the substrate, thereby preparing high-quality compound semiconductor materials. In addition, MOCVD technology can also adjust and control the properties of materials by changing parameters such as the flow rate and temperature of the reactant gas.

[0039] Preferably, in this embodiment, the epitaxial layer comprises, from bottom to top, the following layers disposed on the substrate: a buffer layer, an ohmic contact layer, a first confinement layer, a multiple quantum well layer, a second confinement layer, and a GaP layer.

[0040] Step S200: The epitaxial wafer is cleaned sequentially, and the surface of the GaP layer is roughened.

[0041] Preferably, in this embodiment, step S200 specifically includes:

[0042] Step S210: Immerse the epitaxial wafer in the first cleaning solution and rinse it clean with water;

[0043] The epitaxial wafer was immersed in a second cleaning solution and then rinsed clean with water.

[0044] The first cleaning solution is composed of H2O2, NH4OH, and H2O in a volume ratio of 2:1:1; the second cleaning solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 5:1:1.

[0045] Specifically, in this embodiment, the epitaxial wafer is first soaked in a first cleaning solution for 50 seconds, then rinsed with water for 360 seconds. Next, the epitaxial wafer is soaked in a second cleaning solution for 25 seconds, then rinsed with water for 360 seconds, and finally spun dry to ensure that the surface dirt and back phosphide of the epitaxial wafer are effectively cleaned.

[0046] Step S220 involves using ICP etching technology to etch trenches onto the surface of the GaP layer after the first cleaning process. Specifically, ICP etching is a technique that utilizes inductively coupled plasma for etching. ICP etching is a highly efficient, precise, and pollution-free semiconductor etching process. By using ionized plasma to conduct a chemical reaction, some of the material on the surface is removed, thereby enabling the manufacturing and processing of semiconductor chips.

[0047] ICP etching technology utilizes the energy of inductively coupled plasma to convert gas into ions, which are then used for etching. Specifically, when ignited with a high-frequency spark, some of the Ar working gas is ionized. The resulting electrons and argon ions are accelerated in a high-frequency electromagnetic field, colliding with neutral atoms and ionizing even more working gas, forming plasma gas. The conductive plasma gas, under the influence of a magnetic field, induces a powerful current, generating a large amount of heat energy that further heats the plasma, resulting in ICP discharge.

[0048] Step S300: The roughened epitaxial wafer undergoes a secondary cleaning process, and a SiO2 layer is deposited on the surface of the GaP layer. Preferably, in this embodiment, the thickness of the SiO2 layer is [missing information].

[0049] Preferably, in this embodiment, step S300 specifically includes:

[0050] Step S310: Immerse the epitaxial wafer in a third cleaning solution and rinse it with water.

[0051] The third cleaning solution consists of H₂SO₄, H₂O₂, and H₂O in a volume ratio of 5:1:1. The roughened GaP surface is cleaned using this third cleaning solution, resulting in a cleaner surface and eliminating GaP impurities from remaining in the grooves.

[0052] Step S320: Using RF radio frequency technology, a SiO2 layer is deposited on the surface of the epitaxial wafer based on the second preset parameters;

[0053] The second preset parameters include: radio frequency power of 90W-100W, pressure of 80Pa-100Pa, reactant gases of N2 and SiH4, and SiH4 flow rate of 290sccm-300sccm. Preferably, in this embodiment, the radio frequency power is preferably 100W, the pressure is preferably 90Pa, and the SiH4 flow rate is preferably 300sccm.

[0054] By adjusting the silane flow rate, increasing the chamber pressure, and reducing the power, the compressive stress of SiO2 was increased.

[0055] To make it easier to understand, the aforementioned RF (radio frequency) technology specifically employs plasma-enhanced chemical vapor deposition (PECVD), a thin film fabrication technique widely used in the electronics industry. It utilizes plasma to activate gas molecules, causing a chemical reaction when these molecules interact with a solid surface, thereby forming a thin film. While PECVD is based on chemical vapor deposition (CVD), the introduction of plasma energy can increase the reaction rate, lower the reaction temperature, alter the film composition and structure, and enhance the film's adhesion and density. The active species in the plasma react with the precursor gas to form a thin film on the solid surface.

[0056] The advantage of PECVD lies in its ability to operate at relatively low temperatures, thereby reducing thermal stress on the substrate material. It offers high reaction rates and good controllability, enabling the fabrication of thin films from a variety of materials. This makes PECVD widely used in the electronics industry, including the fabrication of thin-film transistors, solar cells, display devices, and optical thin films. By adjusting parameters such as precursor gas, plasma energy, and reaction conditions, precise control over the composition, structure, and properties of the thin films can be achieved to meet diverse application requirements.

[0057] Step S400: Polish the surface of the SiO2 layer, and then place the polished epitaxial wafer and sapphire into an acidic activation solution for activation treatment. The acidic activation solution consists of H2SO4, H2O2, and H2O in a volume ratio of 7:3:1. Specifically, by preparing the acidic activation solution, hydrogen-oxygen bonds can be effectively suspended on the bonding surfaces of sapphire and SiO2. This facilitates the subsequent bonding process under high temperature and pressure, where two -OH groups remove a water molecule to form -O- bonds, thus bonding SiO2 and sapphire together.

[0058] Furthermore, in some application scenarios of this embodiment, by placing both the sapphire and the epitaxial wafer into the above-mentioned acidic activation solution and letting them stand for 2 minutes, and then rinsing and drying them, compared with the use of alkaline activation solutions such as ammonia in the prior art, the amount of hydrogen-oxygen bonds attached can be increased, and the bonding force can be improved.

[0059] In step S500, the epitaxial wafer and the sapphire after activation are bonded together, and the substrate is removed to obtain a Mini-LED.

[0060] Specifically, in this embodiment, step S500 includes:

[0061] Step S510: Based on the first preset parameters, perform high-temperature bonding between the activated epitaxial wafer and the sapphire.

[0062] The first preset parameters include: bonding pressure of 8000 kgf-12000 kgf, bonding temperature of 400℃-500℃, and bonding time of 900 s-1000 s. Preferably, in some application scenarios of this embodiment, when maintaining the bonded state, the above-mentioned bonding pressure is 10000 kgf (initial pressure of 500 kgf, pressurization rate of 100 kgf / s), the bonding temperature is 450℃ (initial temperature of 150℃, heating rate of 1℃ / s), and the bonding holding time is 900 s. By optimizing the bonding temperature and using high-temperature bonding, the adhesion between sapphire and the epitaxial layer can be improved.

[0063] Step S520: Use a substrate etching solution to etch one side of the substrate of the bonded epitaxial wafer to remove the substrate and expose the epitaxial layer;

[0064] The surface of one side of the epitaxial layer of the epitaxial wafer is cleaned with acetone and isopropanol to obtain Mini-LED.

[0065] Specifically, the substrate etching solution is a mixture of ammonia and hydrogen peroxide. Preferably, the volume ratio of ammonia to hydrogen peroxide in the substrate etching solution is 9:1.

[0066] In summary, the Mini-LED fabrication method in the above embodiments of the present invention, by depositing a SiO2 layer using the second preset parameters, specifically by adjusting the silane flow rate, increasing the chamber pressure, and reducing the power, improves the compressive stress of SiO2, thereby enhancing the adhesion between the SiO2 layer and the sapphire and Gap layers. By optimizing the activation method and eliminating the conventional alkaline activation method, more hydrogen-oxygen bonds are attached to the surfaces of the sapphire and SiO2 layers, thereby improving the bonding effect. Furthermore, by using the first preset parameters to achieve bonding between the sapphire and the SiO2 layer, specifically by employing high-temperature bonding, the adhesion between the sapphire and the epitaxial layer is further increased. Based on the above points, the yield of epitaxial layer transfer onto sapphire is greatly increased, avoiding dimming and dead LED problems caused by epitaxial layer delamination during end-use.

[0067] Example 2

[0068] The second embodiment of the present invention provides a method for fabricating Mini-LEDs. The Mini-LED fabrication method in this embodiment is basically the same as the Mini-LED fabrication method in the first embodiment, except that:

[0069] In this embodiment, the first preset parameters include: a bonding pressure of 8000 kgf, a bonding temperature of 500 °C, and a bonding holding time of 1000 s.

[0070] Example 3

[0071] The third embodiment of the present invention provides a method for fabricating Mini-LEDs. The Mini-LED fabrication method in this embodiment is basically the same as the Mini-LED fabrication method in the first embodiment, except that:

[0072] In this embodiment, the first preset parameters include: a bonding pressure of 9000 kgf, a bonding temperature of 400 °C, and a bonding holding time of 950 s.

[0073] Example 4

[0074] The fourth embodiment of the present invention provides a method for fabricating Mini-LEDs. The Mini-LED fabrication method in this embodiment is basically the same as the Mini-LED fabrication method in the first embodiment, except that:

[0075] In this embodiment, the second preset parameters include: RF power of 90W, pressure of 100Pa, and SiH4 flow rate of 300sccm.

[0076] Example 5

[0077] The fifth embodiment of the present invention provides a method for fabricating Mini-LEDs. The difference between the Mini-LED fabrication method in this embodiment and the Mini-LED fabrication method in the first embodiment is as follows:

[0078] In this embodiment, the second preset parameters include: RF power of 100W, pressure of 80Pa, and SiH4 flow rate of 290sccm.

[0079] Compare with Example 1

[0080] A method for fabricating a Mini-LED includes the following steps:

[0081] Step S1: An epitaxial layer is grown on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on the side away from the substrate;

[0082] Step S2: The epitaxial wafer is cleaned sequentially, and the surface of the GaP layer is roughened.

[0083] Step S3: Perform a secondary cleaning process on the roughened epitaxial wafer, and deposit a SiO2 layer on the surface of the GaP layer;

[0084] Step S4: Polish the surface of the SiO2 layer, and place the polished epitaxial wafer and sapphire into an alkaline activation solution for activation treatment. The alkaline activation solution is composed of NH4OH, H2O2 and H2O in a volume ratio of 7:3:1.

[0085] Step S5: Bond the activated epitaxial wafer and the sapphire together, and remove the substrate to obtain a Mini-LED.

[0086] Specifically, the steps and parameters not mentioned in this comparative example are the same as those in Example 1. The difference is that this method uses an alkaline activating solution for activation treatment.

[0087] Compare with Example 2

[0088] Step S1: An epitaxial layer is grown on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on the side away from the substrate;

[0089] Step S2: The epitaxial wafer is cleaned sequentially, and the surface of the GaP layer is roughened.

[0090] Step S3: Perform a secondary cleaning process on the roughened epitaxial wafer, and deposit a SiO2 layer on the surface of the GaP layer;

[0091] Step S4: Polish the surface of the SiO2 layer, and place the polished epitaxial wafer and sapphire into an acidic activation solution for activation treatment. The acidic activation solution is composed of H2SO4, H2O2 and H2O in a volume ratio of 7:3:1.

[0092] Step S5: Bond the activated epitaxial wafer and the sapphire together, and remove the substrate to obtain a Mini-LED.

[0093] Specifically, in this comparative example, step S3 specifically includes: using RF radio frequency technology and depositing a SiO2 layer on the surface of the epitaxial wafer based on a third preset parameter;

[0094] The third preset parameters include: radio frequency power of 120W, pressure of 60Pa, reaction gases of N2 and SiH4, and SiH4 flow rate of 260sccm.

[0095] Specifically, the steps and parameters not mentioned in this comparative example are the same as those in Example 1. However, the difference is that in this comparative example, for the third preset parameter (corresponding to the first preset parameter in Example 1), the radio frequency power is higher, the pressure is lower, and the flow rate of SiH4 is lower.

[0096] Compare with Example 3

[0097] Step S1: An epitaxial layer is grown on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on the side away from the substrate;

[0098] Step S2: The epitaxial wafer is cleaned sequentially, and the surface of the GaP layer is roughened.

[0099] Step S3: Perform a secondary cleaning process on the roughened epitaxial wafer, and deposit a SiO2 layer on the surface of the GaP layer;

[0100] Step S4: Polish the surface of the SiO2 layer, and place the polished epitaxial wafer and sapphire into an acidic activation solution for activation treatment. The acidic activation solution is composed of H2SO4, H2O2 and H2O in a volume ratio of 7:3:1.

[0101] Step S5: Bond the activated epitaxial wafer and the sapphire together, and remove the substrate to obtain a Mini-LED.

[0102] Specifically, in this comparative example, step S5 specifically includes: performing high-temperature bonding between the activated epitaxial wafer and the sapphire based on the fourth preset parameters;

[0103] The aforementioned fourth preset parameters include: a bonding pressure of 10000 kgf, a bonding holding time of 900 s, and a bonding temperature of 350 °C.

[0104] Specifically, the steps and parameters not mentioned in this comparative example are the same as those in Example 1. However, a comparison reveals that the difference lies in the fact that the bonding temperature in this comparative example is lower for the fourth preset parameter (corresponding to the second preset parameter in Example 1).

[0105] The bonding yield of the products obtained in each of the above embodiments, Comparative Example 1 and Comparative Example 2 was measured. The results are shown in Table 1 below. As can be seen from Table 1, the product yield achieved by each embodiment of this application is 98.5% or higher, which is higher than the product yield obtained by Comparative Example 1 and Comparative Example 2.

[0106] Bonding yield Example 1 98.90% Example 2 98.60% Example 3 98.50% Example 4 98.50% Example 5 98.70% Compare with Example 1 96.30% Compare with Example 2 95.50% Compare with Example 3 95.60% .

[0107] Example 6

[0108] The sixth embodiment of the present invention provides a Mini-LED, which is prepared by the Mini-LED preparation method in the above embodiments.

[0109] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0110] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the appended claims.

Claims

1. A method for fabricating a Mini-LED, characterized in that, Includes the following steps: An epitaxial layer is grown on a substrate to obtain an epitaxial wafer, wherein the epitaxial layer includes a GaP layer disposed on the side away from the substrate; The epitaxial wafer is subjected to a cleaning process once in sequence, and the surface of the GaP layer is roughened. The roughened epitaxial wafer is subjected to a secondary cleaning process, and a SiO2 layer is deposited on the surface of the GaP layer. The surface of the SiO2 layer is polished, and the polished epitaxial wafer and sapphire are placed in an acidic activation solution for activation treatment. The epitaxial wafer and the sapphire crystal after activation treatment are bonded together, and the substrate is removed to obtain a Mini-LED. The acidic activation solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 7:3:1; The specific steps for bonding the activated epitaxial wafer and the sapphire crystal include: Based on the first preset parameters, the activated epitaxial wafer and the sapphire are bonded at high temperature. The first preset parameters include: bonding pressure of 8000 kgf-12000 kgf, bonding temperature of 400℃-500℃, and bonding time of 900 s-1000 s. The thickness of the SiO2 layer is 30,000 Å.

2. The Mini-LED fabrication method according to claim 1, characterized in that, The step of depositing a SiO2 layer on the surface of the epitaxial wafer specifically includes: An RF (radio frequency) technology is used, and a SiO2 layer is deposited on the surface of the epitaxial wafer based on a second preset parameter. The second preset parameters include: radio frequency power of 90W-100W, pressure of 80Pa-100Pa, reaction gases of N2 and SiH4, and SiH4 flow rate of 290sccm-300sccm.

3. The Mini-LED fabrication method according to claim 1, characterized in that, The specific steps of performing a cleaning process on the epitaxial wafer include: The epitaxial wafer is immersed in the first cleaning solution and then rinsed clean with water. The epitaxial wafer was immersed in a second cleaning solution and then rinsed clean with water. The first cleaning solution is composed of H2O2, NH4OH, and H2O in a volume ratio of 2:1:1; the second cleaning solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 5:1:

1.

4. The Mini-LED fabrication method according to claim 3, characterized in that, The specific steps for roughening the surface of the GaP layer include: ICP etching technology is used to etch trenches on the surface of the GaP layer after a first cleaning process.

5. The Mini-LED fabrication method according to claim 1, characterized in that, The specific steps for secondary cleaning of the roughened epitaxial wafer include: The epitaxial wafer was immersed in a third cleaning solution and then rinsed clean with water. The third cleaning solution is composed of H2SO4, H2O2, and H2O in a volume ratio of 5:1:

1.

6. The Mini-LED fabrication method according to claim 1, characterized in that, The step of removing the substrate to obtain the Mini-LED specifically includes: A substrate etching solution is used to etch one side of the substrate of the bonded epitaxial wafer to remove the substrate and expose the epitaxial layer; The surface of one side of the epitaxial layer of the epitaxial wafer is cleaned with acetone and isopropanol to obtain Mini-LED; The substrate etching solution is composed of H2O2 and NH4OH in a volume ratio of 9:

1.

7. A Mini-LED, characterized in that, The Mini-LED is prepared by the Mini-LED preparation method according to any one of claims 1-6.

Citation Information

Patent Citations

  • Method for improving mini LED bonding yield